MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Chromium-Copper, UNS C17600, TH04 Temper rod, bar, wire, tubing, plate
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Applications: resistance welding electrodes for spot, seam, flash, and projection welding methods; electrical connectors, clips

TB00 temper rod, bar, wire, plate, and tubing.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.75 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 95 - 102
Tensile Strength, Ultimate 760 - 900 MPa
Tensile Strength, Yield 690 - 825 MPa
@Strain 0.2 %
Elongation at Break 10 - 20 %
Modulus of Elasticity 125 - 130 GPa
Shear Modulus 44.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000029 - 0.0000034 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.7 µm/m-°C
@Temperature 20.0 - 200 °C
Specific Heat Capacity 0.420 J/g-°C
Thermal Conductivity 215 - 245 W/m-K
Melting Point 1031 - 1068 °C
Solidus 1031 °C
Liquidus 1068 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 975 °CHot-Shortness Temperature
Annealing Temperature 900 - 950 °C10 minutes/water quench
Aging Temperature 425 °C3-6 hours, for maximum strength
 480 °CCommercial practice, 2-3 hours
Hot-Working Temperature 750 - 925 °C
 
Component Elements PropertiesOriginal ValueComments
Beryllium, Be 0.25 - 0.50 %
Co + Ni >= 1.4 %
Co + Ni + Fe <= 1.9 %
Cobalt, Co 1.4 - 1.7 %
Copper, Cu 97 %
Silver, Ag 0.90 - 1.1 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Beryllium Copper, UNS C17300, TB00 Temper rod, bar, plate, tubing
Beryllium Copper, UNS C17300, TD04 Temper rod, bar, plate, tubing, <9.5 mm
Cartridge Brass, UNS C26000 (260 Brass), H06 wire
Beryllium Copper, UNS C17300, TH04 Temper wire, <2 mm
Beryllium Copper, UNS C17300, TH04 Temper rod, bar, plate, tubing, <9.5 mm

MC17600b4 / 10913

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.