MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

JIS SKD12 Tool Steel
Categories: Metal; Ferrous Metal; Tool Steel; Air-Hardening Steel; Cold Work Steel

Material Notes: Medium-Alloy, Air-Hardening Cold Work Tool Steel. High hardenability, high degree of dimensional stability in heat treatment, good wear resistance, fatigue life, toughness, and deep hardening qualities. Applications include cold forming, blanking and bending dies, forming rolls, drill bushings, knurling tools, master dies and gages.

Composition reported is for SKD12 while other property data is from AISI A2.

Key Words: JIS G4404(83) Specification. SKD 12, SKD-12, Comparable to AISI A2, UNS T30102, ASTM A681, FED QQ-T-570, SAE J437, SAE J438, DIN 1.2363, AFNOR Z 100 CDV 5 (Fr), SS14 2260 (Sweden), B.S. BA 2
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.86 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 63 - 65
@Temperature 23.0 °C
63 - 65
@Temperature 73.4 °F
as air-hardened
 42 - 4442 - 44
 50 - 5250 - 52
 56 - 5856 - 58
 58 - 6058 - 60
 58 - 6058 - 60
 58 - 6058 - 60
 58 - 6058 - 60
 59 - 6159 - 61
 60 - 6260 - 62
Modulus of Elasticity 203 GPa29400 ksi
Bulk Modulus 160 GPa23200 ksiTypical for steels.
Poissons Ratio 0.300.30Calculated
Machinability 65 %65 %Based on Carbon tool steel.
Shear Modulus 78.0 GPa11300 ksiEstimated from elastic modulus
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.7 µm/m-°C
@Temperature 20.0 - 100 °C
5.94 µin/in-°F
@Temperature 68.0 - 212 °F
 12.0 µm/m-°C
@Temperature 20.0 - 200 °C
6.67 µin/in-°F
@Temperature 68.0 - 392 °F
 12.7 µm/m-°C
@Temperature 20.0 - 300 °C
7.06 µin/in-°F
@Temperature 68.0 - 572 °F
 13.2 µm/m-°C
@Temperature 20.0 - 400 °C
7.33 µin/in-°F
@Temperature 68.0 - 752 °F
 13.7 µm/m-°C
@Temperature 20.0 - 500 °C
7.61 µin/in-°F
@Temperature 68.0 - 932 °F
 14.0 µm/m-°C
@Temperature 20.0 - 600 °C
7.78 µin/in-°F
@Temperature 68.0 - 1110 °F
 14.3 µm/m-°C
@Temperature 20.0 - 700 °C
7.94 µin/in-°F
@Temperature 68.0 - 1290 °F
 14.4 µm/m-°C
@Temperature 20.0 - 750 °C
8.00 µin/in-°F
@Temperature 68.0 - 1380 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 175 - 540 °C347 - 1000 °FTempering Temperature
 925 - 980 °C1700 - 1800 °FHardening Temperature
Annealing Temperature 845 - 870 °C1550 - 1600 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.95 - 1.05 %0.95 - 1.05 %
Chromium, Cr 4.5 - 5.5 %4.5 - 5.5 %
Iron, Fe 90.8 - 92.9 %90.8 - 92.9 %As Balance
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Molybdenum, Mo 0.80 - 1.2 %0.80 - 1.2 %
Silicon, Si 0.40 %0.40 %
Vanadium, V 0.20 - 0.50 %0.20 - 0.50 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type A2 Tool Steel
Bohler-Uddeholm SUPERIOR® H13 Hot Work Tool Steel
Bohler-Uddeholm AISI A2 Cold Work Tool Steel
JIS S45C Steel, Normalized
AISI Type D2 Tool Steel, air quenched at 1010°C, tempered at 200°C

MSTZJSKD12 / 231068

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.