MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Bohler-Uddeholm SUPERIOR® H13 Hot Work Tool Steel  (discontinued **)
Categories: Metal; Ferrous Metal; Alloy Steel; Tool Steel; Hot Work Steel

Material Notes:

This premium H13 grade steel, produced via special melting and refining techniques possesses excellent toughness making it suitable for demanding hot work applications. W302 Superior meets or exceeds NADCA 207-97 and 207-2003 Superior Specification in dimensions 18" and greater in thickness.

A premium grade H13 hot work tool steel featuring:

  • Very good toughness properties
  • Very good heat checking resistance
  • Good temper resistance and high temperature strength
  • Excellent polishability and texturability
  • Manufactured for flats greater than 18 inches in thickness

Key Words: DIN 1.2344; JIS SKD61; 40CrMoV5
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.81 g/cc0.282 lb/in³
 7.61 g/cc
@Temperature 593 °C
0.275 lb/in³
@Temperature 1100 °F
 7.64 g/cc
@Temperature 499 °C
0.276 lb/in³
@Temperature 930 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 53531870°F, 30 min Soak
 54541920°F, 15 min Soak
Tensile Strength, Ultimate  359 MPa
@Temperature 649 °C
52000 psi
@Temperature 1200 °F
treated to 175 ksi)
 586 MPa
@Temperature 649 °C
85000 psi
@Temperature 1200 °F
treated to 230 ksi)
 1100 MPa
@Temperature 316 °C
160000 psi
@Temperature 600 °F
treated to 175 ksi)
 1380 MPa
@Temperature 316 °C
200000 psi
@Temperature 600 °F
treated to 230 ksi)
Tensile Strength, Yield  331 MPa
@Strain 0.2 %,
Temperature 649 °C
48000 psi
@Strain 0.2 %,
Temperature 1200 °F
Heat treated to 175 ksi
 414 MPa
@Strain 0.2 %,
Temperature 649 °C
60000 psi
@Strain 0.2 %,
Temperature 1200 °F
Heat treated to 230 ksi
 896 MPa
@Strain 0.2 %,
Temperature 316 °C
130000 psi
@Strain 0.2 %,
Temperature 600 °F
Heat treated to 175 ksi
 1170 MPa
@Strain 0.2 %,
Temperature 316 °C
170000 psi
@Strain 0.2 %,
Temperature 600 °F
Heat treated to 230 ksi
Reduction of Area  50 %
@Temperature 316 °C
50 %
@Temperature 600 °F
Heat treated to 175 ksi
 50 %
@Temperature 316 °C
50 %
@Temperature 600 °F
Heat treated to 230 ksi
 55 %
@Temperature 649 °C
55 %
@Temperature 1200 °F
Heat treated to 230 ksi
 90 %
@Temperature 649 °C
90 %
@Temperature 1200 °F
Heat treated to 175 ksi
Modulus of Elasticity 215 GPa31200 ksi
 165 GPa
@Temperature 593 °C
23900 ksi
@Temperature 1100 °F
 176 GPa
@Temperature 499 °C
25500 ksi
@Temperature 930 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000520 ohm-cm0.0000520 ohm-cm
 0.0000860 ohm-cm
@Temperature 499 °C
0.0000860 ohm-cm
@Temperature 930 °F
 0.0000960 ohm-cm
@Temperature 593 °C
0.0000960 ohm-cm
@Temperature 1100 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.5 µm/m-°C
@Temperature 93.3 °C
6.40 µin/in-°F
@Temperature 200 °F
 12.4 µm/m-°C
@Temperature 399 °C
6.90 µin/in-°F
@Temperature 750 °F
 13.1 µm/m-°C
@Temperature 704 °C
7.30 µin/in-°F
@Temperature 1300 °F
Specific Heat Capacity 0.460 J/g-°C0.110 BTU/lb-°F
 0.548 J/g-°C
@Temperature 499 °C
0.131 BTU/lb-°F
@Temperature 930 °F
 0.590 J/g-°C
@Temperature 593 °C
0.141 BTU/lb-°F
@Temperature 1100 °F
Thermal Conductivity 25.0 W/m-K174 BTU-in/hr-ft²-°Fhardened
 26.8 W/m-K186 BTU-in/hr-ft²-°Fannealed
 27.7 W/m-K
@Temperature 399 °C
192 BTU-in/hr-ft²-°F
@Temperature 750 °F
hardened
 30.4 W/m-K
@Temperature 704 °C
211 BTU-in/hr-ft²-°F
@Temperature 1300 °F
hardened
 31.0 W/m-K
@Temperature 399 °C
215 BTU-in/hr-ft²-°F
@Temperature 750 °F
annealed
 33.4 W/m-K
@Temperature 704 °C
232 BTU-in/hr-ft²-°F
@Temperature 1300 °F
annealed
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.39 %0.39 %
Chromium, Cr 5.2 %5.2 %
Iron, Fe 90.56 %90.56 %As Balance
Manganese, Mn 0.40 %0.40 %
Molybdenum, Mo 1.4 %1.4 %
Silicon, Si 1.1 %1.1 %
Sulfur, S <= 0.0030 %<= 0.0030 %
Vanadium, V 0.95 %0.95 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type H13 Hot Work Tool Steel
Bohler-Uddeholm BÖHLER W302 ISOBLOC® H13 hot work tool steel
AISI E 52100 Steel (100Cr6, SUJ2, UNS G52986)
Bohler-Uddeholm ISOBLOC® H13 Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel

NBUCOR09 / 15478

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.