MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes 188 alloy, plate at RT after 8000 hours at 650°C (1200°F)
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Excellent high temperature strength and very good resistance to oxidizing environments up to 1095°C for prolonged exposure, and excellent resistance to sulfate deposit hot corrosion. Readily fabricated and formed, excellent resistance to molten chloride salts, and good resistance to gaseous sulfidation. Applications include a variety of fabricated component applications in the aerospace industry, commercial gas turbine engines for combustion cans, transition ducts and afterburner components.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS R30188, AMS 5608, AMS 5772, AMS 5801
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.98 g/ccat RT.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 1045 MPa
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
Elongation at Break 29.1 %in 51 mm
Modulus of Elasticity 232 GPaRT
 153 GPa
@Temperature 1000 °C
 161 GPa
@Temperature 900 °C
 169 GPa
@Temperature 800 °C
 176 GPa
@Temperature 700 °C
 184 GPa
@Temperature 600 °C
 193 GPa
@Temperature 500 °C
 201 GPa
@Temperature 400 °C
 209 GPa
@Temperature 300 °C
 217 GPa
@Temperature 200 °C
 225 GPa
@Temperature 100 °C
Charpy Impact 31.0 Jafter 8000 hours at 650°C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000101 ohm-cmRT
 0.000103 ohm-cm
@Temperature 100 °C
 0.000105 ohm-cm
@Temperature 200 °C
 0.0001077 ohm-cm
@Temperature 300 °C
 0.0001105 ohm-cm
@Temperature 400 °C
 0.0001127 ohm-cm
@Temperature 500 °C
 0.0001148 ohm-cm
@Temperature 600 °C
 0.0001164 ohm-cm
@Temperature 700 °C
 0.0001175 ohm-cm
@Temperature 800 °C
 0.0001183 ohm-cm
@Temperature 900 °C
 0.0001191 ohm-cm
@Temperature 1000 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.9 µm/m-°C
@Temperature 25.0 - 100 °C
 12.6 µm/m-°C
@Temperature 25.0 - 200 °C
 13.2 µm/m-°C
@Temperature 25.0 - 300 °C
 13.8 µm/m-°C
@Temperature 25.0 - 400 °C
 14.5 µm/m-°C
@Temperature 25.0 - 500 °C
 15.2 µm/m-°C
@Temperature 25.0 - 600 °C
 15.8 µm/m-°C
@Temperature 25.0 - 700 °C
 16.5 µm/m-°C
@Temperature 25.0 - 800 °C
 17.1 µm/m-°C
@Temperature 25.0 - 800 °C
 17.9 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.403 J/g-°CRT
 0.423 J/g-°C
@Temperature 100 °C
 0.444 J/g-°C
@Temperature 200 °C
 0.465 J/g-°C
@Temperature 300 °C
 0.486 J/g-°C
@Temperature 400 °C
 0.502 J/g-°C
@Temperature 500 °C
 0.523 J/g-°C
@Temperature 600 °C
 0.540 J/g-°C
@Temperature 700 °C
 0.557 J/g-°C
@Temperature 800 °C
 0.573 J/g-°C
@Temperature 900 °C
 0.590 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 10.4 W/m-KRT
 12.2 W/m-K
@Temperature 100 °C
 14.3 W/m-K
@Temperature 200 °C
 15.9 W/m-K
@Temperature 300 °C
 17.5 W/m-K
@Temperature 400 °C
 19.3 W/m-K
@Temperature 500 °C
 21.1 W/m-K
@Temperature 600 °C
 23.0 W/m-K
@Temperature 700 °C
 24.8 W/m-K
@Temperature 800 °C
 25.5 W/m-K
@Temperature 900 °C
 27.6 W/m-K
@Temperature 1000 °C
Melting Point 1315 - 1410 °C
Solidus 1315 °C
Liquidus 1410 °C
Maximum Service Temperature, Air 1095 °C
 
Component Elements PropertiesOriginal ValueComments
Boron, B <= 0.015 %
Carbon, C 0.050 - 0.15 %
Chromium, Cr 21 - 23 %
Cobalt, Co 42 %As remainder
Iron, Fe <= 3.0 %
Lanthanum, La 0.020 - 0.12 %
Manganese, Mn <= 1.25 %
Nickel, Ni 20 - 24 %
Silicon, Si 0.20 - 0.50 %
Tungsten, W 13 - 15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Haynes 188 alloy, hot rolled and 1175°C solution annealed plate
CoCrWNi Alloy, ASTM F90
CoCrMoWNi Alloy, ASTM F563
Haynes 188 alloy, plate at RT after 8000 hours at 760°C (1400°F)
S-816 Cobalt Alloy, UNS R30816

NH18AR / 16372

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.