MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 188 alloy, hot rolled and 1175°C solution annealed plate
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Excellent high temperature strength and very good resistance to oxidizing environments up to 1095°C for prolonged exposure, and excellent resistance to sulfate deposit hot corrosion. Readily fabricated and formed, excellent resistance to molten chloride salts, and good resistance to gaseous sulfidation. Applications include a variety of fabricated component applications in the aerospace industry, commercial gas turbine engines for combustion cans, transition ducts and afterburner components.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS R30188, AMS 5608, AMS 5772, AMS 5801
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.98 g/cc0.324 lb/in³at RT.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 985 MPa143000 psi
 83.0 MPa
@Temperature 1205 °C
12000 psi
@Temperature 2201 °F
 96.0 MPa
@Temperature 1150 °C
13900 psi
@Temperature 2100 °F
 145 MPa
@Temperature 1095 °C
21000 psi
@Temperature 2003 °F
 265 MPa
@Temperature 980 °C
38400 psi
@Temperature 1800 °F
 450 MPa
@Temperature 870 °C
65300 psi
@Temperature 1600 °F
 650 MPa
@Temperature 760 °C
94300 psi
@Temperature 1400 °F
 755 MPa
@Temperature 650 °C
110000 psi
@Temperature 1200 °F
 775 MPa
@Temperature 540 °C
112000 psi
@Temperature 1000 °F
Tensile Strength, Yield 470 MPa
@Strain 0.2 %
68200 psi
@Strain 0.2 %
 28.0 MPa
@Strain 0.2 %,
Temperature 1205 °C
4060 psi
@Strain 0.2 %,
Temperature 2201 °F
 48.0 MPa
@Strain 0.2 %,
Temperature 1150 °C
6960 psi
@Strain 0.2 %,
Temperature 2100 °F
 88.0 MPa
@Strain 0.2 %,
Temperature 1095 °C
12800 psi
@Strain 0.2 %,
Temperature 2003 °F
 185 MPa
@Strain 0.2 %,
Temperature 980 °C
26800 psi
@Strain 0.2 %,
Temperature 1800 °F
 250 MPa
@Strain 0.2 %,
Temperature 870 °C
36300 psi
@Strain 0.2 %,
Temperature 1600 °F
 265 MPa
@Strain 0.2 %,
Temperature 650 °C
38400 psi
@Strain 0.2 %,
Temperature 1200 °F
 270 MPa
@Strain 0.2 %,
Temperature 760 °C
39200 psi
@Strain 0.2 %,
Temperature 1400 °F
 275 MPa
@Strain 0.2 %,
Temperature 540 °C
39900 psi
@Strain 0.2 %,
Temperature 1000 °F
Elongation at Break 56 %56 %in 51 mm
 60 %
@Temperature 1150 °C
60 %
@Temperature 2100 °F
in 51 mm
 69 %
@Temperature 540 °C
69 %
@Temperature 1000 °F
in 51 mm
 70 %
@Temperature 760 °C
70 %
@Temperature 1400 °F
in 51 mm
 71 %
@Temperature 1205 °C
71 %
@Temperature 2201 °F
in 51 mm
 73 %
@Temperature 650 °C
73 %
@Temperature 1200 °F
in 51 mm
 77 %
@Temperature 870 °C
77 %
@Temperature 1600 °F
in 51 mm
 84 %
@Temperature 980 °C
84 %
@Temperature 1800 °F
in 51 mm
 89 %
@Temperature 1095 °C
89 %
@Temperature 2003 °F
in 51 mm
Modulus of Elasticity 232 GPa33600 ksiRT
 153 GPa
@Temperature 1000 °C
22200 ksi
@Temperature 1830 °F
 161 GPa
@Temperature 900 °C
23400 ksi
@Temperature 1650 °F
 169 GPa
@Temperature 800 °C
24500 ksi
@Temperature 1470 °F
 176 GPa
@Temperature 700 °C
25500 ksi
@Temperature 1290 °F
 184 GPa
@Temperature 600 °C
26700 ksi
@Temperature 1110 °F
 193 GPa
@Temperature 500 °C
28000 ksi
@Temperature 932 °F
 201 GPa
@Temperature 400 °C
29200 ksi
@Temperature 752 °F
 209 GPa
@Temperature 300 °C
30300 ksi
@Temperature 572 °F
 217 GPa
@Temperature 200 °C
31500 ksi
@Temperature 392 °F
 225 GPa
@Temperature 100 °C
32600 ksi
@Temperature 212 °F
Charpy Impact 194 J143 ft-lbsolution annealed
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000101 ohm-cm0.000101 ohm-cmRT
 0.000103 ohm-cm
@Temperature 100 °C
0.000103 ohm-cm
@Temperature 212 °F
 0.000105 ohm-cm
@Temperature 200 °C
0.000105 ohm-cm
@Temperature 392 °F
 0.0001077 ohm-cm
@Temperature 300 °C
0.0001077 ohm-cm
@Temperature 572 °F
 0.0001105 ohm-cm
@Temperature 400 °C
0.0001105 ohm-cm
@Temperature 752 °F
 0.0001127 ohm-cm
@Temperature 500 °C
0.0001127 ohm-cm
@Temperature 932 °F
 0.0001148 ohm-cm
@Temperature 600 °C
0.0001148 ohm-cm
@Temperature 1110 °F
 0.0001164 ohm-cm
@Temperature 700 °C
0.0001164 ohm-cm
@Temperature 1290 °F
 0.0001175 ohm-cm
@Temperature 800 °C
0.0001175 ohm-cm
@Temperature 1470 °F
 0.0001183 ohm-cm
@Temperature 900 °C
0.0001183 ohm-cm
@Temperature 1650 °F
 0.0001191 ohm-cm
@Temperature 1000 °C
0.0001191 ohm-cm
@Temperature 1830 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.9 µm/m-°C
@Temperature 25.0 - 100 °C
6.61 µin/in-°F
@Temperature 77.0 - 212 °F
 12.6 µm/m-°C
@Temperature 25.0 - 200 °C
7.00 µin/in-°F
@Temperature 77.0 - 392 °F
 13.2 µm/m-°C
@Temperature 25.0 - 300 °C
7.33 µin/in-°F
@Temperature 77.0 - 572 °F
 13.8 µm/m-°C
@Temperature 25.0 - 400 °C
7.67 µin/in-°F
@Temperature 77.0 - 752 °F
 14.5 µm/m-°C
@Temperature 25.0 - 500 °C
8.06 µin/in-°F
@Temperature 77.0 - 932 °F
 15.2 µm/m-°C
@Temperature 25.0 - 600 °C
8.44 µin/in-°F
@Temperature 77.0 - 1110 °F
 15.8 µm/m-°C
@Temperature 25.0 - 700 °C
8.78 µin/in-°F
@Temperature 77.0 - 1290 °F
 16.5 µm/m-°C
@Temperature 25.0 - 800 °C
9.17 µin/in-°F
@Temperature 77.0 - 1470 °F
 17.1 µm/m-°C
@Temperature 25.0 - 800 °C
9.50 µin/in-°F
@Temperature 77.0 - 1470 °F
 17.9 µm/m-°C
@Temperature 25.0 - 1000 °C
9.94 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.403 J/g-°C0.0963 BTU/lb-°FRT
 0.423 J/g-°C
@Temperature 100 °C
0.101 BTU/lb-°F
@Temperature 212 °F
 0.444 J/g-°C
@Temperature 200 °C
0.106 BTU/lb-°F
@Temperature 392 °F
 0.465 J/g-°C
@Temperature 300 °C
0.111 BTU/lb-°F
@Temperature 572 °F
 0.486 J/g-°C
@Temperature 400 °C
0.116 BTU/lb-°F
@Temperature 752 °F
 0.502 J/g-°C
@Temperature 500 °C
0.120 BTU/lb-°F
@Temperature 932 °F
 0.523 J/g-°C
@Temperature 600 °C
0.125 BTU/lb-°F
@Temperature 1110 °F
 0.540 J/g-°C
@Temperature 700 °C
0.129 BTU/lb-°F
@Temperature 1290 °F
 0.557 J/g-°C
@Temperature 800 °C
0.133 BTU/lb-°F
@Temperature 1470 °F
 0.573 J/g-°C
@Temperature 900 °C
0.137 BTU/lb-°F
@Temperature 1650 °F
 0.590 J/g-°C
@Temperature 1000 °C
0.141 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 10.4 W/m-K72.2 BTU-in/hr-ft²-°FRT
 12.2 W/m-K
@Temperature 100 °C
84.7 BTU-in/hr-ft²-°F
@Temperature 212 °F
 14.3 W/m-K
@Temperature 200 °C
99.2 BTU-in/hr-ft²-°F
@Temperature 392 °F
 15.9 W/m-K
@Temperature 300 °C
110 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.5 W/m-K
@Temperature 400 °C
121 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.3 W/m-K
@Temperature 500 °C
134 BTU-in/hr-ft²-°F
@Temperature 932 °F
 21.1 W/m-K
@Temperature 600 °C
146 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 23.0 W/m-K
@Temperature 700 °C
160 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.8 W/m-K
@Temperature 800 °C
172 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 25.5 W/m-K
@Temperature 900 °C
177 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 27.6 W/m-K
@Temperature 1000 °C
192 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1315 - 1410 °C2399 - 2570 °F
Solidus 1315 °C2399 °F
Liquidus 1410 °C2570 °F
Maximum Service Temperature, Air 1095 °C2003 °F
 
Component Elements PropertiesMetricEnglishComments
Boron, B <= 0.015 %<= 0.015 %
Carbon, C 0.050 - 0.15 %0.050 - 0.15 %
Chromium, Cr 21 - 23 %21 - 23 %
Cobalt, Co 42 %42 %As remainder
Iron, Fe <= 3.0 %<= 3.0 %
Lanthanum, La 0.020 - 0.12 %0.020 - 0.12 %
Manganese, Mn <= 1.25 %<= 1.25 %
Nickel, Ni 20 - 24 %20 - 24 %
Silicon, Si 0.20 - 0.50 %0.20 - 0.50 %
Tungsten, W 13 - 15 %13 - 15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Universal Wire Works Haynes 188 (AMS 5801) Filler Metal
Haynes 188 alloy, cold rolled and 1175°C solution annealed sheet
CoCrWNi Alloy, ASTM F90
Haynes 188 alloy, plate at RT after 8000 hours at 650°C (1200°F)
CoCrMoWNi Alloy, ASTM F563

NH18AH / 16362

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.