MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

X-40 Cobalt Alloy (UNS R30031)
Categories: Metal; Nonferrous Metal; Cobalt Alloy

Material Notes: Typical applications: gas turbine parts, nozzle vanes

Key Words: HS-31
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.60 g/cc0.311 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Rupture Strength  27.6 MPa
@Temperature 1090 °C,
Time 360000 sec
4000 psi
@Temperature 2000 °F,
Time 100 hour
 27.6 MPa
@Temperature 1090 °C,
Time 360000 sec
4000 psi
@Temperature 2000 °F,
Time 100 hour
 55.2 MPa
@Temperature 982 °C,
Time 3.60e+6 sec
8000 psi
@Temperature 1800 °F,
Time 1000 hour
 55.2 MPa
@Temperature 982 °C,
Time 3.60e+6 sec
8000 psi
@Temperature 1800 °F,
Time 1000 hour
 75.8 MPa
@Temperature 982 °C,
Time 360000 sec
11000 psi
@Temperature 1800 °F,
Time 100 hour
 75.8 MPa
@Temperature 982 °C,
Time 360000 sec
11000 psi
@Temperature 1800 °F,
Time 100 hour
 138 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
20000 psi
@Temperature 1500 °F,
Time 1000 hour
 138 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
20000 psi
@Temperature 1500 °F,
Time 1000 hour
 179 MPa
@Temperature 816 °C,
Time 360000 sec
26000 psi
@Temperature 1500 °F,
Time 100 hour
 179 MPa
@Temperature 816 °C,
Time 360000 sec
26000 psi
@Temperature 1500 °F,
Time 100 hour
 338 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
49000 psi
@Temperature 1200 °F,
Time 1000 hour
 338 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
49000 psi
@Temperature 1200 °F,
Time 1000 hour
 393 MPa
@Temperature 649 °C,
Time 360000 sec
57000 psi
@Temperature 1200 °F,
Time 100 hour
 393 MPa
@Temperature 649 °C,
Time 360000 sec
57000 psi
@Temperature 1200 °F,
Time 100 hour
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.50 %0.50 %
Chromium, Cr 25 %25 %
Cobalt, Co 54 %54 %
Nickel, Ni 10 %10 %
Tungsten, W 7.5 %7.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
QuesTek® Innovations Ferrium® S53® Corrosion Resistant High Strength Steel for Aerospace Structural Applications
MetalTek MTEK 31 UNS R30031 Cobalt Base Alloy
Cobalt Titanium 94Co-6Ti Alloy
Cobalt, Co
Cobalt Samarium 3 Hard Magnetic Alloy

NZ978 / 170628

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.