MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
INEOS Styrolution Polystyrol 495 F GR 2 PS
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene, Impact Modified

Material Notes: Styrolution PS 495N is an impact resistant polystyrene with a good balance of toughness, high flow, heat resistance and high gloss. High flow, Good balance of toughness and heat resistance. Applications: Injection molding, TV & office equipment components, Air conditioners, Water tanks for toilet flushing.

Information provided by STYROLUTION, which is a joint venture between BASF and INEOS

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccISO 1183
Moisture Absorption at Equilibrium <= 0.10 %
@Temperature 23.0 °C
50% RH; ISO 62
Water Absorption at Saturation <= 0.10 %
@Temperature 23.0 °C
ISO 62
Linear Mold Shrinkage 0.0030 - 0.0060 cm/cmISO 294-4
Melt Flow 9.5 g/10 min
@Load 5.00 kg,
Temperature 200 °C
Volumetric; cm3/10 min; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 74.0 MPaISO 2039-1
Tensile Strength, Yield 26.0 MPaISO 527
Elongation at Break 40 %ISO 527
Elongation at Yield 1.5 %ISO 527
Tensile Modulus 2000 MPaISO 527
Flexural Strength 40.0 MPaISO 178
Flexural Modulus 2100 MPaISO 178
Izod Impact, Notched 180 J/mASTM D256
Izod Impact, Notched (ISO) 13.0 kJ/m²
@Temperature 23.0 °C
ISO 180/A
Charpy Impact Unnotched 130 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 17.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+18 ohm-cmIEC 60093
Surface Resistance >= 1.00e+13 ohmIEC 60093
Dielectric Constant 2.5
@Frequency 100 Hz
IEC 60250
 2.5
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.00040
@Frequency 100 Hz
IEC 60250
 0.00040
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear 100 µm/m-°CISO 11359
Thermal Conductivity 0.170 W/m-KDIN 52612-1
Deflection Temperature at 0.46 MPa (66 psi) 89.0 °Cannealed 4 hours at 80°C; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °Cannealed 4 hours at 80°C; ISO 75
Vicat Softening Point 90.0 °C
@Load 5.10 kg
VST/B/50. 50C/h; ISO 306
 98.0 °C
@Load 1.02 kg
VST/A/50. 50C/h; ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 180 - 260 °CISO 294
Mold Temperature 10.0 - 60.0 °CISO 294
Injection Velocity 200 mm/secISO 294
 
Descriptive Properties
ColorNatural
Commercial StatusEurope
Primary Processing TechniqueInjection Molding
Surface Gloss45Skalenteile

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
INEOS Styrolution PS 495F HIPS
KKPC Kuhmo HI 450S High Gloss HIPS
Arkema KYNAR® 370 Polyvinylidene Fluoride (PVDF) Homopolymer - Injection Molding
BASF Polystyrol® 432 B Impact Grade Polystyrene (Europe)
Chi Mei Polyrex® PH-60 Polystyrene - High Impact

PBASG0632 / 132265

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.