MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 5182-H34
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A95182; Aluminium 5182-H34; AA5182-H34; Al5182-H34
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.65 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 91500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 115Converted from Brinell Hardness Value
Hardness, Rockwell A 38.5Converted from Brinell Hardness Value
Hardness, Rockwell B 57Converted from Brinell Hardness Value
Hardness, Vickers 102Converted from Brinell Hardness Value
Tensile Strength, Ultimate 340 MPa
Tensile Strength, Yield 240 MPa
Elongation at Break 10 %
@Thickness 1.60 mm
In 5 cm
Tensile Modulus 69.6 GPa
Compressive Modulus 70.9 GPa
Poissons Ratio 0.33
Shear Modulus 26.0 GPaCalculated
Shear Strength 200 MPaCalculated value.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000560 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 22.2 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.9 µm/m-°C
@Temperature 20.0 - 100 °C
 24.1 µm/m-°C
@Temperature 20.0 - 100 °C
 25.0 µm/m-°C
@Temperature 20.0 - 200 °C
 26.0 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.904 J/g-°C
Thermal Conductivity 126 W/m-K
Melting Point 577 - 638 °C
Solidus 577 °C
Liquidus 638 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 650 °F
Hot-Working Temperature 500 - 950 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 93.2 - 95.8 %As remainder
Chromium, Cr <= 0.10 %
Copper, Cu <= 0.15 %
Iron, Fe <= 0.35 %
Magnesium, Mg 4.0 - 5.0 %
Manganese, Mn 0.20 - 0.50 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti <= 0.10 %
Zinc, Zn <= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 5182-H32
Aluminum 5182-H19
Aluminum 5182-O
Aluminum 3104-H19
Aluminum 6061-T6; 6061-T651

MA5182H34 / 9219

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.