MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 5182-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A95182; Aluminium 5182-O; AA5182-O; Al5182-O
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.65 g/cc0.0957 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 7474500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 9797Converted from Brinell Hardness Value
Hardness, Vickers 8484Converted from Brinell Hardness Value
Tensile Strength, Ultimate 275 MPa39900 psi
Tensile Strength, Yield 130 MPa18900 psi
Elongation at Break 21 %
@Thickness 1.60 mm
21 %
@Thickness 0.0630 in
In 5 cm
Tensile Modulus 69.6 GPa10100 ksi
Compressive Modulus 70.9 GPa10300 ksi
Poissons Ratio 0.330.33
Fatigue Strength 138 MPa
@# of Cycles 5.00e+8
20000 psi
@# of Cycles 5.00e+8
Shear Modulus 26.0 GPa3770 ksiCalculated
Shear Strength 150 MPa21800 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000560 ohm-cm0.00000560 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  22.2 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.3 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.9 µm/m-°C
@Temperature 20.0 - 100 °C
13.3 µin/in-°F
@Temperature 68.0 - 212 °F
 24.1 µm/m-°C
@Temperature 20.0 - 100 °C
13.4 µin/in-°F
@Temperature 68.0 - 212 °F
 25.0 µm/m-°C
@Temperature 20.0 - 200 °C
13.9 µin/in-°F
@Temperature 68.0 - 392 °F
 26.0 µm/m-°C
@Temperature 20.0 - 300 °C
14.4 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.904 J/g-°C0.216 BTU/lb-°F
Thermal Conductivity 126 W/m-K874 BTU-in/hr-ft²-°F
Melting Point 577 - 638 °C1070 - 1180 °F
Solidus 577 °C1070 °F
Liquidus 638 °C1180 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 343 °C650 °F
Hot-Working Temperature 260 - 510 °C500 - 950 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 93.2 - 95.8 %93.2 - 95.8 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu <= 0.15 %<= 0.15 %
Iron, Fe <= 0.35 %<= 0.35 %
Magnesium, Mg 4.0 - 5.0 %4.0 - 5.0 %
Manganese, Mn 0.20 - 0.50 %0.20 - 0.50 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti <= 0.10 %<= 0.10 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5182-H32
Aluminum 5182-H19
Aluminum 5182-H34
Aluminum 5052-O
5754-H22 Aluminum

MA5182O / 9220

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.