Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.20 g/cc | 1.20 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 71 | 71 |
| 58 @Treatment Temp. 23.0 °C, Time 252000 sec | 58 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 61 @Treatment Temp. 23.0 °C, Time 252000 sec | 61 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 65 @Treatment Temp. 125 °C, Time 252000 sec | 65 @Treatment Temp. 257 °F, Time 70.0 hour |
| 65 @Treatment Temp. 150 °C, Time 252000 sec | 65 @Treatment Temp. 302 °F, Time 70.0 hour |
| 66 @Treatment Temp. 100 °C, Time 252000 sec | 66 @Treatment Temp. 212 °F, Time 70.0 hour |
| 71 @Treatment Temp. 100 °C, Time 252000 sec | 71 @Treatment Temp. 212 °F, Time 70.0 hour |
| 71 @Treatment Temp. 23.0 °C, Time 252000 sec | 71 @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 73 @Treatment Temp. 150 °C, Time 252000 sec | 73 @Treatment Temp. 302 °F, Time 70.0 hour |
| 73 @Treatment Temp. 100 °C, Time 252000 sec | 73 @Treatment Temp. 212 °F, Time 70.0 hour |
| 73 @Treatment Temp. 125 °C, Time 252000 sec | 73 @Treatment Temp. 257 °F, Time 70.0 hour |
| 75 @Treatment Temp. 100 °C, Time 252000 sec | 75 @Treatment Temp. 212 °F, Time 70.0 hour |
| 77 @Treatment Temp. 125 °C, Time 252000 sec | 77 @Treatment Temp. 257 °F, Time 70.0 hour |
| 77 @Treatment Temp. 100 °C, Time 252000 sec | 77 @Treatment Temp. 212 °F, Time 70.0 hour |
| 81 @Treatment Temp. 100 °C, Time 252000 sec | 81 @Treatment Temp. 212 °F, Time 70.0 hour |
| 81 @Treatment Temp. 150 °C, Time 252000 sec | 81 @Treatment Temp. 302 °F, Time 70.0 hour |
Tensile Strength | 20.64 MPa | 2993 psi |
| 0.390 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 56.6 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 8.6053 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1248.1 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 12.155 MPa @Treatment Temp. 23.0 °C, Time 252000 sec | 1762.9 psi @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 15.995 MPa @Treatment Temp. 125 °C, Time 252000 sec | 2319.9 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 17.396 MPa @Treatment Temp. 100 °C, Time 252000 sec | 2523.1 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 17.396 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2523.1 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 19.893 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2885.3 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 20.718 MPa @Treatment Temp. 125 °C, Time 252000 sec | 3004.9 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 20.780 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3013.9 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 20.925 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3034.9 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 21.276 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3085.8 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 21.441 MPa @Treatment Temp. 125 °C, Time 252000 sec | 3109.7 psi @Treatment Temp. 257 °F, Time 70.0 hour |
| 21.441 MPa @Treatment Temp. 100 °C, Time 252000 sec | 3109.7 psi @Treatment Temp. 212 °F, Time 70.0 hour |
| 21.544 MPa @Treatment Temp. 150 °C, Time 252000 sec | 3124.7 psi @Treatment Temp. 302 °F, Time 70.0 hour |
Elongation, Ultimate | 307 % | 307 % |
| 146.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 146.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 206 % @Treatment Temp. 23.0 °C, Time 252000 sec | 206 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 264.9 % @Treatment Temp. 150 °C, Time 252000 sec | 264.9 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 264.9 % @Treatment Temp. 100 °C, Time 252000 sec | 264.9 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 307 % @Treatment Temp. 100 °C, Time 252000 sec | 307 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 307 % @Treatment Temp. 125 °C, Time 252000 sec | 307 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 310.07 % @Treatment Temp. 23.0 °C, Time 252000 sec | 310.07 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 311.9 % @Treatment Temp. 100 °C, Time 252000 sec | 311.9 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 318.1 % @Treatment Temp. 125 °C, Time 252000 sec | 318.1 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 337.1 % @Treatment Temp. 100 °C, Time 252000 sec | 337.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 337.1 % @Treatment Temp. 100 °C, Time 252000 sec | 337.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 337.1 % @Treatment Temp. 125 °C, Time 252000 sec | 337.1 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 337.1 % @Treatment Temp. 150 °C, Time 252000 sec | 337.1 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 338.9 % @Treatment Temp. 150 °C, Time 252000 sec | 338.9 % @Treatment Temp. 302 °F, Time 70.0 hour |
100% Modulus | 4.10 MPa | 594 psi |
Tear Strength | 40.8 kN/m | 233 pli |
| 51.4 kN/m | 293 pli |
Compression Set | 11.5 % @Treatment Temp. 100 °C, Time 79200 sec | 11.5 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 11.6 % @Treatment Temp. 125 °C, Time 79200 sec | 11.6 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 11.6 % @Treatment Temp. 100 °C, Time 79200 sec | 11.6 % @Treatment Temp. 212 °F, Time 22.0 hour |
| 12.6 % @Treatment Temp. 125 °C, Time 79200 sec | 12.6 % @Treatment Temp. 257 °F, Time 22.0 hour |
| 15 % @Treatment Temp. 100 °C, Time 252000 sec | 15 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 15.2 % @Treatment Temp. 150 °C, Time 79200 sec | 15.2 % @Treatment Temp. 302 °F, Time 22.0 hour |
| 16 % @Treatment Temp. 100 °C, Time 252000 sec | 16 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 16.6 % @Treatment Temp. 150 °C, Time 79200 sec | 16.6 % @Treatment Temp. 302 °F, Time 22.0 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -38.9 °C | -38.0 °F |
Shrinkage | -3.70 % @Treatment Temp. 150 °C, Time 252000 sec | -3.70 % @Treatment Temp. 302 °F, Time 70.0 hour |
| -3.60 % @Treatment Temp. 125 °C, Time 252000 sec | -3.60 % @Treatment Temp. 257 °F, Time 70.0 hour |
| -3.40 % @Treatment Temp. 100 °C, Time 252000 sec | -3.40 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 0.30 % @Treatment Temp. 100 °C, Time 252000 sec | 0.30 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 4.1 % @Treatment Temp. 23.0 °C, Time 252000 sec | 4.1 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 12.5 % @Treatment Temp. 100 °C, Time 252000 sec | 12.5 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 12.9 % @Treatment Temp. 125 °C, Time 252000 sec | 12.9 % @Treatment Temp. 257 °F, Time 70.0 hour |
| 14 % @Treatment Temp. 150 °C, Time 252000 sec | 14 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 36.7 % @Treatment Temp. 23.0 °C, Time 252000 sec | 36.7 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
| 58.6 % @Treatment Temp. 23.0 °C, Time 252000 sec | 58.6 % @Treatment Temp. 73.4 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |