MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum Martensitic Stainless Steel Type 440A, Hardened + 427°C Temper
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Allegheny Ludlum Type 440A is a hardenable straight-chromium stainless steel which combines superior wear resistance of high carbon alloys with the excellent corrosion resistance of chromium stainless steels. Oil quenching this alloy from temperatures between 1800°F and 1950°F produces the high strength and/or wear resistance as well as corrosion resistance.

A major use for this grade of heat treatable stainless steel is in cutlery. Type 440A is not readily amenable to fine blanking due to its higher strength and hardness in the annealed condition; and therefore, could require more powerful presses to blank parts. In addition, the presence of large primary carbides in Type 440A would tend to reduce die life.

UTS, TYS, and hardness values below obtained after austenitizing at 1800-1950°F (982-1066°C) followed by an oil quench and two hour temper.

Information provided by Allegheny Ludlum Corporation.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.74 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 53
Tensile Strength, Ultimate 1881 MPaTypical
Tensile Strength, Yield 1610 MPa
@Strain 0.2 %
typical
Modulus of Elasticity 200 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000620 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 15.0 µm/m-°C
@Temperature 20.0 - 200 °C
 16.8 µm/m-°C
@Temperature 20.0 - 600 °C
Thermal Conductivity 24.207 W/m-K
@Temperature 100 °C
Melting Point 1399 - 1510 °C
Solidus 1399 °C
Liquidus 1510 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.60 - 0.75 %
Chromium, Cr 16 - 18 %
Iron, Fe 81 %as balance
Manganese, Mn <= 1.0 %
Molybdenum, Mo <= 0.75 %
Nickel, Ni <= 0.50 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum Martensitic Stainless Steel Type 440A, Hardened + 316°C Temper
ATI Allegheny Ludlum Martensitic Stainless Steel Type 440A, Hardened + 204°C Temper
ATI Allegheny Ludlum Martensitic Stainless Steel Type 440A, Hardened + 288°C Temper
ATI Allegheny Ludlum Martensitic Stainless Steel Type 440A, Hardened + 482°C Temper
AIM 35.7Sn/35.7Pb/28.6Bi Solder for Photonic Packaging

NL4404 / 17945

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.