MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Pressure Seal 5747 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 5747 is a 70 durometer black colored Buna N. It is on the Underwriter Laboratories approved list for use with gasoline, kerosene, fuel oils, LP Gas, Naptha, manufactured and natural gas, and anhydrous ammonia. This compound exhibits a good balance of properties. The working temperature range for this compound is -20°F to 212°F with intermittent peaks to 250°F.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 715 B14 B34; 2 BG 715 B14 B34 EA14 EF11 EF21; 5 BG 715 A14 B14 B34 EO14; 4 BK 715 B14 B34 EF11 EF21

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.34 g/cc1.34 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7171
 52
@Treatment Temp. 150 °C,
Time 252000 sec
52
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
 59
@Treatment Temp. 23.0 °C,
Time 252000 sec
59
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 61
@Treatment Temp. 23.0 °C,
Time 252000 sec
61
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Unleaded Gas (89 Octane): Aged
 62
@Treatment Temp. 65.0 °C,
Time 252000 sec
62
@Treatment Temp. 149 °F,
Time 70.0 hour
Methanol: Aged
 63
@Treatment Temp. 23.0 °C,
Time 252000 sec
63
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 70
@Treatment Temp. 23.0 °C,
Time 605000 sec
70
@Treatment Temp. 73.4 °F,
Time 168 hour
MAPP Gas: Aged
 70
@Treatment Temp. 100 °C,
Time 252000 sec
70
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 74
@Treatment Temp. 100 °C,
Time 252000 sec
74
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3
 79
@Treatment Temp. 125 °C,
Time 252000 sec
79
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 81
@Treatment Temp. 100 °C,
Time 252000 sec
81
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1
 81
@Treatment Temp. 150 °C,
Time 252000 sec
81
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 82
@Treatment Temp. 100 °C,
Time 252000 sec
82
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
 87
@Treatment Temp. 125 °C,
Time 252000 sec
87
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 88
@Treatment Temp. 125 °C,
Time 252000 sec
88
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
 88
@Treatment Temp. 125 °C,
Time 252000 sec
88
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
Tensile Strength 11.33 MPa1644 psi
 6.710 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
973.2 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 6.801 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
986.4 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 9.8616 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
1430.3 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 10.168 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
1474.7 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
 10.201 MPa
@Treatment Temp. 70.0 °C,
Time 346000 sec
1479.6 psi
@Treatment Temp. 158 °F,
Time 96.0 hour
Oxygen Bomb: Aged
 10.258 MPa
@Treatment Temp. 65.0 °C,
Time 252000 sec
1487.8 psi
@Treatment Temp. 149 °F,
Time 70.0 hour
Methanol: Aged
 10.258 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1487.8 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Unleaded Gas (89 Octane): Aged
 10.8589 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1574.95 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 10.961 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
1589.7 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 11.097 MPa
@Treatment Temp. 23.0 °C,
Time 605000 sec
1609.5 psi
@Treatment Temp. 73.4 °F,
Time 168 hour
MAPP Gas: Aged
 11.496 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
1667.3 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
 11.516 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
1670.3 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 11.856 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
1719.6 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3
 11.924 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
1729.5 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1
 12.060 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
1749.2 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 12.333 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
1788.7 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
HEXANE: Aged
 13.398 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
1943.2 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 14.350 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
2081.3 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
Elongation, Ultimate 360 %360 %
 159.84 %
@Treatment Temp. 150 °C,
Time 252000 sec
159.84 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
 240.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
240.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged
 240.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
240.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Heat Aged, Test Tube Method
 249.8 %
@Treatment Temp. 125 °C,
Time 252000 sec
249.8 %
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #1
 270 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
270 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Liquid Anhydrous Ammonia: Aged
 270 %
@Treatment Temp. 125 °C,
Time 252000 sec
270 %
@Treatment Temp. 257 °F,
Time 70.0 hour
ASTM Oil #3
 295.56 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
295.56 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Unleaded Gas (89 Octane): Aged
 295.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
295.6 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
HEXANE: Aged
 299.88 %
@Treatment Temp. 100 °C,
Time 252000 sec
299.88 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 307.08 %
@Treatment Temp. 150 °C,
Time 252000 sec
307.08 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 309.96 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
309.96 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel B
 309.96 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
309.96 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 309.96 %
@Treatment Temp. 100 °C,
Time 252000 sec
309.96 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
 317.88 %
@Treatment Temp. 100 °C,
Time 252000 sec
317.88 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1
 325.8 %
@Treatment Temp. 65.0 °C,
Time 252000 sec
325.8 %
@Treatment Temp. 149 °F,
Time 70.0 hour
Methanol: Aged
 330.84 %
@Treatment Temp. 100 °C,
Time 252000 sec
330.84 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3
 334.4 %
@Treatment Temp. 70.0 °C,
Time 346000 sec
334.4 %
@Treatment Temp. 158 °F,
Time 96.0 hour
Oxygen Bomb: Aged
 356.04 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
356.04 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel A
 377.3 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
377.3 %
@Treatment Temp. 73.4 °F,
Time 168 hour
MAPP Gas: Aged
100% Modulus 3.21 MPa466 psi
Tear Strength 18.9 kN/m108 pliDie C
 41.4 kN/m236 pliDie B
Compression Set  7.5 %
@Treatment Temp. 100 °C,
Time 79200 sec
7.5 %
@Treatment Temp. 212 °F,
Time 22.0 hour
Solid
 7.6 %
@Treatment Temp. 125 °C,
Time 79200 sec
7.6 %
@Treatment Temp. 257 °F,
Time 22.0 hour
Solid
 9.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
9.9 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Solid
 17 %
@Treatment Temp. 125 °C,
Time 79200 sec
17 %
@Treatment Temp. 257 °F,
Time 22.0 hour
Plied
 18.6 %
@Treatment Temp. 100 °C,
Time 79200 sec
18.6 %
@Treatment Temp. 212 °F,
Time 22.0 hour
Plied
 19 %
@Treatment Temp. 100 °C,
Time 252000 sec
19 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Plied
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -28.9 °C-20.0 °F
Shrinkage  -10.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
-10.7 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 -10.3 %
@Treatment Temp. 125 °C,
Time 252000 sec
-10.3 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 -7.40 %
@Treatment Temp. 100 °C,
Time 252000 sec
-7.40 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 -2.10 %
@Treatment Temp. 125 °C,
Time 252000 sec
-2.10 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 -1.70 %
@Treatment Temp. 100 °C,
Time 252000 sec
-1.70 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 -1.50 %
@Treatment Temp. 150 °C,
Time 252000 sec
-1.50 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 -0.900 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
-0.900 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel A
 0.90 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
0.90 %
@Treatment Temp. 73.4 °F,
Time 168 hour
MAPP Gas: Aged
 2.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
2.2 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, HEXANE: Aged
 4.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
4.6 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, Liquid Anhydrous Ammonia: Aged
 6.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
6.4 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, Distilled water aged
 9.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
9.9 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Unleaded Gas (89 Octane): Aged
 9.9 %
@Treatment Temp. 65.0 °C,
Time 252000 sec
9.9 %
@Treatment Temp. 149 °F,
Time 70.0 hour
Volume, Methanol: Aged
 14.7 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
14.7 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel B
 24.4 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
24.4 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack
TR-10 Temperature-18°FASTM D1329 (10% Retraction)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL042 / 318252

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.