MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 5747 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 5747 is a 70 durometer black colored Buna N. It is on the Underwriter Laboratories approved list for use with gasoline, kerosene, fuel oils, LP Gas, Naptha, manufactured and natural gas, and anhydrous ammonia. This compound exhibits a good balance of properties. The working temperature range for this compound is -20°F to 212°F with intermittent peaks to 250°F.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 715 B14 B34; 2 BG 715 B14 B34 EA14 EF11 EF21; 5 BG 715 A14 B14 B34 EO14; 4 BK 715 B14 B34 EF11 EF21

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.34 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 71
 52
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
 59
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 61
@Treatment Temp. 23.0 °C,
Time 252000 sec
Unleaded Gas (89 Octane): Aged
 62
@Treatment Temp. 65.0 °C,
Time 252000 sec
Methanol: Aged
 63
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 70
@Treatment Temp. 23.0 °C,
Time 605000 sec
MAPP Gas: Aged
 70
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 74
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 79
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 81
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 81
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 82
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 87
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 88
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 88
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 1644 psi
 973.2 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 986.4 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 1430.3 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 1474.7 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 1479.6 psi
@Treatment Temp. 70.0 °C,
Time 346000 sec
Oxygen Bomb: Aged
 1487.8 psi
@Treatment Temp. 65.0 °C,
Time 252000 sec
Methanol: Aged
 1487.8 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
Unleaded Gas (89 Octane): Aged
 1574.95 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1589.7 psi
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 1609.5 psi
@Treatment Temp. 23.0 °C,
Time 605000 sec
MAPP Gas: Aged
 1667.3 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 1670.3 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1719.6 psi
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 1729.5 psi
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 1749.2 psi
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 1788.7 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
HEXANE: Aged
 1943.2 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 2081.3 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
Elongation, Ultimate 360 %
 159.84 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
 240.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 240.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 249.8 %
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 270 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Liquid Anhydrous Ammonia: Aged
 270 %
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 295.56 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Unleaded Gas (89 Octane): Aged
 295.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
HEXANE: Aged
 299.88 %
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 307.08 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 309.96 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 309.96 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 309.96 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 317.88 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 325.8 %
@Treatment Temp. 65.0 °C,
Time 252000 sec
Methanol: Aged
 330.84 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 334.4 %
@Treatment Temp. 70.0 °C,
Time 346000 sec
Oxygen Bomb: Aged
 356.04 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 377.3 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
MAPP Gas: Aged
100% Modulus 466 psi
Tear Strength 108 pliDie C
 236 pliDie B
Compression Set 7.5 %
@Treatment Temp. 100 °C,
Time 79200 sec
Solid
 7.6 %
@Treatment Temp. 125 °C,
Time 79200 sec
Solid
 9.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
Solid
 17 %
@Treatment Temp. 125 °C,
Time 79200 sec
Plied
 18.6 %
@Treatment Temp. 100 °C,
Time 79200 sec
Plied
 19 %
@Treatment Temp. 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -20.0 °F
Shrinkage -10.7 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -10.3 %
@Treatment Temp. 125 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -7.40 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -2.10 %
@Treatment Temp. 125 °C,
Time 252000 sec
Volume, ASTM Oil #3
 -1.70 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 -1.50 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 -0.900 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.90 %
@Treatment Temp. 23.0 °C,
Time 605000 sec
MAPP Gas: Aged
 2.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, HEXANE: Aged
 4.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, Liquid Anhydrous Ammonia: Aged
 6.4 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 9.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Unleaded Gas (89 Octane): Aged
 9.9 %
@Treatment Temp. 65.0 °C,
Time 252000 sec
Volume, Methanol: Aged
 14.7 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 24.4 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack
TR-10 Temperature-18°FASTM D1329 (10% Retraction)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL042 / 318252

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.