(Viewing data as-entered.
Click here
to return)
Dow PELLETHANE® 2101-85A Polyurethane Elastomer (Ether-Ether Hybrid)
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Elastomer, TPE
;
Polyurethane, TP
;
Thermoplastic Polyurethane, Elastomer, Ether Grade
Material Notes:
Description:
PELLETHANE® 2101-85A offers good low temperature properties, fast cycle time, and good hydrolytic stability. Applications include: seals, gaskets, animal tags, molding applications, hose jacket.
Data provided by Dow Chemical.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
1.13
g/cc
ASTM D792
Melt Index of Compound
45
g/10 min
@Load 1.20 kg,
Temperature 224 °C
ASTM D1238
Mechanical Properties
Original Value
Comments
Hardness, Shore A
84 - 92
ASTM D2240
Tensile Strength, Ultimate
28.0
MPa
ASTM D412
Elongation at Break
590 %
ASTM D412
100% Modulus
0.00800
GPa
@Strain 100 %
ASTM D412
300% Modulus
0.0129
GPa
@Strain 300 %
ASTM D412
Tear Strength
111
kN/m
Die C; ASTM D624
Taber Abrasion, mg/1000 Cycles
40
H-22 wheel (coarser); ASTM D1044
Compression Set
81 %
@Temperature 70.0 °C
22 hrs.; ASTM D395, Method B
Tensile Set
120 %
Elongation Set After Break; ASTM D412
Thermal Properties
Original Value
Comments
Vicat Softening Point
109
°C
ASTM D1525
Glass Transition Temp, Tg
-24.0
°C
DSC
Processing Properties
Original Value
Comments
Melt Temperature
204
-
221
°C
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Huntsman IROGRAN® A 95 P 5044 DP TPU-Polyether
Lubrizol Pellethane® 2363-65D Thermoplastic Polyurethane Elastomer
Lubrizol Pellethane® 2363-80A Thermoplastic Polyurethane Elastomer
Dow Pellethane® 2103-90AEF Polyurethane Elastomer, Ether Based
BASF Elastollan® 1190A Polyether Type Polyurethane Elastomer
PDW292 / 34460
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.