MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

416 Stainless Steel
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes: 25 mm diameter bar, oil quenched from 995°C, held at tempering temperature for 2 hours.

Key Words: UNS S41600, ASME SA194, ASTM A194, ASTM A314, ASTM A473, ASTM A581, ASTM A582, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405(51416), DIN 1.4005, UNI X 12 CrS 13, B.S. 416 S 21, martensitic, ISO 683/13 7
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  237
@Temperature 705 °C
237
@Temperature 1300 °F
Converted from Rockwell C Hardness
 253
@Temperature 650 °C
253
@Temperature 1200 °F
Converted from Rockwell C Hardness
 266
@Temperature 595 °C
266
@Temperature 1100 °F
Converted from Rockwell C Hardness
 318
@Temperature 540 °C
318
@Temperature 1000 °F
Converted from Rockwell C Hardness
 360
@Temperature 260 °C
360
@Temperature 500 °F
Converted from Rockwell C Hardness
 360
@Temperature 370 °C
360
@Temperature 698 °F
Converted from Rockwell C Hardness
 360
@Temperature 480 °C
360
@Temperature 896 °F
Converted from Rockwell C Hardness
 365
@Temperature 150 °C
365
@Temperature 302 °F
Converted from Rockwell C Hardness
Hardness, Knoop  250
@Temperature 705 °C
250
@Temperature 1300 °F
Converted from Rockwell C Hardness
 268
@Temperature 650 °C
268
@Temperature 1200 °F
Converted from Rockwell C Hardness
 283
@Temperature 595 °C
283
@Temperature 1100 °F
Converted from Rockwell C Hardness
 343
@Temperature 540 °C
343
@Temperature 1000 °F
Converted from Rockwell C Hardness
 392
@Temperature 260 °C
392
@Temperature 500 °F
Converted from Rockwell C Hardness
 392
@Temperature 370 °C
392
@Temperature 698 °F
Converted from Rockwell C Hardness
 392
@Temperature 480 °C
392
@Temperature 896 °F
Converted from Rockwell C Hardness
 397
@Temperature 150 °C
397
@Temperature 302 °F
Converted from Rockwell C Hardness
Hardness, Rockwell C  20
@Temperature 705 °C
20
@Temperature 1300 °F
 23.5
@Temperature 650 °C
23.5
@Temperature 1200 °F
 26
@Temperature 595 °C
26
@Temperature 1100 °F
 34
@Temperature 540 °C
34
@Temperature 1000 °F
 39
@Temperature 260 °C
39
@Temperature 500 °F
 39
@Temperature 370 °C
39
@Temperature 698 °F
 39
@Temperature 480 °C
39
@Temperature 896 °F
 39.5
@Temperature 150 °C
39.5
@Temperature 302 °F
Hardness, Vickers  242
@Temperature 705 °C
242
@Temperature 1300 °F
Converted from Rockwell C Hardness
 260
@Temperature 650 °C
260
@Temperature 1200 °F
Converted from Rockwell C Hardness
 275
@Temperature 595 °C
275
@Temperature 1100 °F
Converted from Rockwell C Hardness
 332
@Temperature 540 °C
332
@Temperature 1000 °F
Converted from Rockwell C Hardness
 378
@Temperature 260 °C
378
@Temperature 500 °F
Converted from Rockwell C Hardness
 378
@Temperature 370 °C
378
@Temperature 698 °F
Converted from Rockwell C Hardness
 378
@Temperature 480 °C
378
@Temperature 896 °F
Converted from Rockwell C Hardness
 383
@Temperature 150 °C
383
@Temperature 302 °F
Converted from Rockwell C hardness.
Tensile Strength, Ultimate  741 MPa
@Temperature 705 °C
107000 psi
@Temperature 1300 °F
 796 MPa
@Temperature 650 °C
115000 psi
@Temperature 1200 °F
 865 MPa
@Temperature 595 °C
125000 psi
@Temperature 1100 °F
 1080 MPa
@Temperature 540 °C
157000 psi
@Temperature 1000 °F
 1185 MPa
@Temperature 480 °C
171900 psi
@Temperature 896 °F
 1260 MPa
@Temperature 370 °C
183000 psi
@Temperature 698 °F
 1295 MPa
@Temperature 260 °C
187800 psi
@Temperature 500 °F
 1310 MPa
@Temperature 150 °C
190000 psi
@Temperature 302 °F
Tensile Strength, Yield  600 MPa
@Strain 0.2 %,
Temperature 705 °C
87000 psi
@Strain 0.2 %,
Temperature 1300 °F
 670 MPa
@Strain 0.2 %,
Temperature 650 °C
97200 psi
@Strain 0.2 %,
Temperature 1200 °F
 740 MPa
@Strain 0.2 %,
Temperature 595 °C
107000 psi
@Strain 0.2 %,
Temperature 1100 °F
 895 MPa
@Strain 0.2 %,
Temperature 540 °C
130000 psi
@Strain 0.2 %,
Temperature 1000 °F
 962 MPa
@Strain 0.2 %,
Temperature 150 °C
140000 psi
@Strain 0.2 %,
Temperature 302 °F
 962 MPa
@Strain 0.2 %,
Temperature 260 °C
140000 psi
@Strain 0.2 %,
Temperature 500 °F
 962 MPa
@Strain 0.2 %,
Temperature 370 °C
140000 psi
@Strain 0.2 %,
Temperature 698 °F
 983 MPa
@Strain 0.2 %,
Temperature 480 °C
143000 psi
@Strain 0.2 %,
Temperature 896 °F
Elongation at Break  9.0 %
@Temperature 150 °C
9.0 %
@Temperature 302 °F
in 50 mm
 9.5 %
@Temperature 260 °C
9.5 %
@Temperature 500 °F
in 50 mm
 13 %
@Temperature 540 °C
13 %
@Temperature 1000 °F
in 50 mm
 14 %
@Temperature 370 °C
14 %
@Temperature 698 °F
in 50 mm
 16 %
@Temperature 480 °C
16 %
@Temperature 896 °F
in 50 mm
 17 %
@Temperature 595 °C
17 %
@Temperature 1100 °F
in 50 mm
 17.5 %
@Temperature 650 °C
17.5 %
@Temperature 1200 °F
in 50 mm
 20 %
@Temperature 705 °C
20 %
@Temperature 1300 °F
in 50 mm
Modulus of Elasticity 200 GPa29000 ksi
Poissons Ratio 0.200.20Calculated
Shear Modulus 83.0 GPa12000 ksi
Izod Impact  20.3 J
@Temperature 150 °C
15.0 ft-lb
@Temperature 302 °F
 20.3 J
@Temperature 260 °C
15.0 ft-lb
@Temperature 500 °F
 20.3 J
@Temperature 370 °C
15.0 ft-lb
@Temperature 698 °F
 20.3 J
@Temperature 480 °C
15.0 ft-lb
@Temperature 896 °F
 27.3 J
@Temperature 540 °C
20.1 ft-lb
@Temperature 1000 °F
 54.4 J
@Temperature 595 °C
40.1 ft-lb
@Temperature 1100 °F
 61.1 J
@Temperature 650 °C
45.1 ft-lb
@Temperature 1200 °F
 75.0 J
@Temperature 705 °C
55.3 ft-lb
@Temperature 1300 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000570 ohm-cm
@Temperature 20.0 °C
0.0000570 ohm-cm
@Temperature 68.0 °F
 0.000108 ohm-cm
@Temperature 650 °C
0.000108 ohm-cm
@Temperature 1200 °F
Magnetic Permeability 700 - 1000700 - 1000annealed condition at RT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.90 µm/m-°C
@Temperature 0.000 - 100 °C
5.50 µin/in-°F
@Temperature 32.0 - 212 °F
 11.0 µm/m-°C
@Temperature 0.000 - 315 °C
6.11 µin/in-°F
@Temperature 32.0 - 599 °F
 11.5 µm/m-°C
@Temperature 0.000 - 540 °C
6.39 µin/in-°F
@Temperature 32.0 - 1000 °F
 11.7 µm/m-°C
@Temperature 0.000 - 650 °C
6.50 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity  24.9 W/m-K
@Temperature 100 °C
173 BTU-in/hr-ft²-°F
@Temperature 212 °F
 28.7 W/m-K
@Temperature 500 °C
199 BTU-in/hr-ft²-°F
@Temperature 932 °F
Melting Point 1480 - 1530 °C2700 - 2790 °F
Solidus 1480 °C2700 °F
Liquidus 1530 °C2790 °F
Maximum Service Temperature, Air 675 °C1250 °FContinuous Service
 760 °C1400 °FIntermittent
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.15 %<= 0.15 %
Chromium, Cr 13 %13 %
Iron, Fe 84 %84 %
Manganese, Mn <= 1.25 %<= 1.25 %
Molybdenum, Mo <= 0.60 %<= 0.60 %
Phosphorus, P <= 0.060 %<= 0.060 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S >= 0.15 %>= 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
410 Stainless Steel
416 Stainless Steel, annealed bar
416 Stainless Steel, tempered bar
AISI 303 Cast Stainless Steel, ASTM A582
302 Stainless Steel, annealed strip

MQ416A / 13035

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.