MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Thermal Ceramics Kaowool S Blanket Strip
Categories: Ceramic; Oxide; Silicon Oxide

Material Notes: Thermal Ceramics Kaowool® Strip products are cut from either Kaowool Blanket, Blanket S, Cerablanket®, or Cerachem® Blanket. These products are available in many forms and lengths depending upon the application. They have low thermal conductivity, low heat storage capacity, and are extremely resistant to thermal shock.

Blanket strip products are highly efficient insulators. These products have low shot content which allows more usable fiber for each insulating dollar. Blanket strip products have longer fibers which give them high tensile strength and resiliency to withstand vibration and physical abuse. Blanket strip products are self-supporting and will not separate, sag, or settle.

Blanket strips are available in a wide variety of widths, thicknesses, densities, and chemistries. This allows the user to select the proper product form for an application with a minimum of scrap and labor to install the strip. Blanket strip products have a wide variety of uses including packing for modules, expansion joints, and gaskets.

Features:

  • Available in a wide variety of widths, thicknesses, and densities
  • Available in all Blanket compositions
  • Applications:

  • Expansion joints
  • High-temperature filtration
  • Gaskets
  • Acoustical service for missiles, rockets, and jet engines
  • High-temperature insulation
  • Packing strips
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.0480 - 0.128 g/cc0.00173 - 0.00462 lb/in³
    Thickness 12500 - 50000 microns492 - 1970 mil
     
    Thermal PropertiesMetricEnglishComments
    Melting Point 1760 °C3200 °F
    Maximum Service Temperature, Air 1090 °C2000 °FContinuous
     1090 °C2000 °FRating
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 35 - 45 %35 - 45 %
    Other 0.00 - 3.0 %0.00 - 3.0 %
    SiO2 50 - 55 %50 - 55 %
    ZrO2 0.00 - 15 %0.00 - 15 %
     
    Descriptive Properties
    MgO Contenttrace
    Water Leachable Elements on Surface of Fiber, PPMBoron, 40
     Chlorine, <10
     Fluorine, <5
     Silicate, 125
     Sodium, 40
     Sulfur, 10

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Morgan Advanced Ceramics Kaowool 80 Organic RCF Vacuum Formed Thermal Ceramic
    Morgan Advanced Ceramics Kaowool 3000 Organic RCF Vacuum Formed Thermal Ceramic
    Morgan Advanced Ceramics Kaowool 2600 Organic RCF Vacuum Formed Thermal Ceramic
    Morgan Advanced Ceramics Green Glass Paper Thermal Ceramic
    Morgan Advanced Ceramics Ceramic Fiber Papers STD Paper Ceramic Fiber

    CTHERM009 / 2329

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.