MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Sandvik 19.12.3.L Welding wire
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: Sandvik 19.12.3.L is a filler material for joining stainless CrNiMo and CrNi steels, stabilized or non-stabilized, e.g. ASTM 316, 316L and 316Ti as well as 304, 304L, 321 and 347, used for service temperatures up to 400 C (750 F), stainless Cr steels with max 19% Cr. Sandvik 19.12.3.L is available as wire and rods for MIG/MAG, TIG, plasma arc and submerged arc welding.

Note 1: Data is typical for non heat treated all-weld metal made by SAW and flux 15W.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 160160
Tensile Strength, Ultimate 580 MPa84100 psiSAW typical for non heat treated weld metal using flux 15W
 470 MPa
@Temperature 400 °C
68200 psi
@Temperature 752 °F
 610 MPa
@Temperature 20.0 °C
88500 psi
@Temperature 68.0 °F
Tensile Strength, Yield 390 MPa
@Strain 0.2 %
56600 psi
@Strain 0.2 %
SAW typical for non heat treated weld metal using flux 15W
 290 MPa
@Strain 0.2 %,
Temperature 400 °C
42100 psi
@Strain 0.2 %,
Temperature 752 °F
 410 MPa
@Strain 0.2 %,
Temperature 20.0 °C
59500 psi
@Strain 0.2 %,
Temperature 68.0 °F
Elongation at Break 35 %35 %SAW typical for non heat treated weld metal using flux 15W
 26 %
@Temperature 400 °C
26 %
@Temperature 752 °F
 35 %
@Temperature 20.0 °C
35 %
@Temperature 68.0 °F
Reduction of Area 40 %40 %
Charpy Impact 60.0 J44.3 ft-lbSAW typical for non heat treated weld metal using flux 15W
 50.0 J
@Temperature -196 °C
36.9 ft-lb
@Temperature -321 °F
 110 J
@Temperature 20.0 °C
81.1 ft-lb
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity  15.0 W/m-K
@Temperature 20.0 °C
104 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 16.0 W/m-K
@Temperature 100 °C
111 BTU-in/hr-ft²-°F
@Temperature 212 °F
 19.0 W/m-K
@Temperature 300 °C
132 BTU-in/hr-ft²-°F
@Temperature 572 °F
 20.0 W/m-K
@Temperature 500 °C
139 BTU-in/hr-ft²-°F
@Temperature 932 °F
Maximum Service Temperature, Air 400 °C752 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.015 %0.015 %All-Weld metal
 0.018 %0.018 %Note 1
 <= 0.020 %<= 0.020 %AIM
Chromium, Cr 18 %18 %Note 1
 18.5 %18.5 %AIM
 18.5 %18.5 %All-Weld metal
Manganese, Mn 1.5 %1.5 %Note 1
 1.8 %1.8 %AIM
 1.8 %1.8 %All-Weld metal
Molybdenum, Mo 2.6 %2.6 %AIM
 2.6 %2.6 %All-Weld metal
 2.6 %2.6 %Note 1
Nickel, Ni 12 %12 %All-Weld metal
 12 %12 %Note 1
 12.5 %12.5 %AIM
Nitrogen, N 0.050 %0.050 %
 0.060 %0.060 %
 <= 0.060 %<= 0.060 %
Phosphorus, P 0.012 %0.012 %All-Weld metal
 0.023 %0.023 %Note 1
 <= 0.025 %<= 0.025 %AIM
Silicon, Si 0.30 %0.30 %All-Weld metal
 0.40 %0.40 %AIM
 0.50 %0.50 %Note 1
Sulfur, S <= 0.015 %<= 0.015 %AIM
 0.10 %0.10 %All-Weld metal
 0.11 %0.11 %Note 1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Schmolz + Bickenbach UGIMA® 316/316L Stainless Steel Bar
Sandvik Kanthal SW 801 Spray wire
Sandvik 19.9.NbR Covered electrodes
AISI Type 316L Stainless Steel, annealed sheet

NSANDV5080 / 199644

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.