MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Dow Engage® 8452 Polyolefin Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Elastomer, Melt-Processible Rubber

Material Notes: Description: Engage® 8452 polyolefin elastomer is an ethyleneoctene copolymer that offers excellent toughness, softness, and optical properties. It has excellent compatibility with other polyolefins, allowing for efficient blending and coextrusion. Engage® 8452 provides excellent flow properties and is efficiently cross-linked by peroxide, silane, or irradiation. When cross-linked, it gives exceptional heat aging, compression set, and weather resistance properties. The product form is free-flowing pellets.

Information provided by manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.875 g/cc0.0316 lb/in³ASTM D792
Mooney Viscosity 11
@Temperature 121 °C
11
@Temperature 250 °F
ML 1 + 4; ASTM D1646
Melt Index of Compound 3.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
3.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7777ASTM D2240
Hardness, Shore D 2525ASTM D2240
Tensile Strength, Ultimate 9.80 MPa1420 psi508 mm/min; ASTM D638
Tensile Strength, Yield 2.50 MPa363 psi508 mm/min; ASTM D638
Elongation at Break 920 %920 %508 mm/min; ASTM D638
2% Secant Modulus 0.0166 GPa2.41 ksiASTM D790
 
Thermal PropertiesMetricEnglishComments
Melting Point 67.0 °C153 °FDSC, 10°C/min; DuPont Test
Vicat Softening Point 43.0 °C109 °FASTM D1525
Brittleness Temperature <= -76.0 °C<= -105 °FASTM D746
 
Descriptive Properties
Comonomer Content35 wt%Dow Method (13C NMR/FTIR)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow Engage® 8842 Polyolefin Elastomer
Dow Engage® 8411 Polyolefin Elastomer
Dow Engage® 8003 Polyolefin Elastomer
Dow Engage® 8130 Polyolefin Elastomer
Dow Engage® 8150 Polyolefin Elastomer

PDVE43 / 34104

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.