MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

ExxonMobil LD 617.LN Molding, Extrusion and Compounding Resin  (discontinued **)
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Molded

Material Notes: Product Description: LD 617.LN is a high flow, low density polyethylene homopolymer resin designed to provide excellent processability, flexibility and surface appearance. This multipurpose resin is performance engineered for applications such as housewares, overcaps and closures and concentrates.

Availability: Latin America, North America and South America

Additive:

  • Antiblock: No
  • Slip: No
  • Thermal Stabilizer: No
Applications:
  • Caps
  • Closures
  • Compounding
  • Food Packaging Containers
  • Houseware Articles
  • Injection Molding
  • Labware
  • Masterbatch Base Resin
Information provided by ExxonMobil Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.919 g/cc0.0332 lb/in³ExxonMobil Method
Melt Flow 26 g/10 min
@Load 2.16 kg,
Temperature 190 °C
26 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 868615s; ASTM D2240
Hardness, Shore D 424215s; ASTM D2240
Tensile Strength at Break 7.58 MPa1100 psiASTM D638
Tensile Strength, Yield 11.0 MPa1600 psiASTM D638
Elongation at Break 120 %120 %ASTM D638
Elongation at Yield 30 %30 %ASTM D638
Flexural Modulus, 1% Secant 234 MPa34000 psiASTM D790
Instrumented Impact Total Energy  16.3 J
@Temperature 22.8 °C
12.0 ft-lb
@Temperature 73.0 °F
ASTM D3763
 19.0 J
@Temperature -20.0 °C
14.0 ft-lb
@Temperature -4.00 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Melting Point 110 °C230 °FPeak Melting Temperature; ExxonMobil Method
Vicat Softening Point 83.9 °C183 °FASTM D1525

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil LD 637.LI Molding, Extrusion and Compounding Resin
ExxonMobil LD 516.LN Molding, Extrusion and Compounding Resin
Celanese 193 LDPE polymer for adhesives, automotive and compounds
ExxonMobil PP4031E2 Polypropylene Impact Copolymer
ExxonMobil PP7011L1 Polypropylene Impact Copolymer

PEXB057 / 37362

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.