MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Vicone High Performance Rubber VicoSil™ KC605Q-OR High Performance Silicone Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE); Silicone; Silicone Rubber

Material Notes: Anti-fungal grade 1 (GB/T 2423.16-2008). RoHS Approved.

Information provided by Vicone

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.166 g/cc0.04212 lb/in³ASTM D3165
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5454ASTM D2240
 59.0
@Treatment Temp. 200 °C,
Time 252000 sec
59.0
@Treatment Temp. 392 °F,
Time 70.0 hour
Heat Aging; ASTM D573
Tensile Strength, Yield 8.00 MPa1160 psiASTM D412
 6.30 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
914 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Heat Aging; ASTM D573
Elongation at Break 551.6 %551.6 %ASTM D412
 346 %
@Treatment Temp. 200 °C,
Time 252000 sec
346 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Heat Aging; ASTM D573
Compressive Modulus  0.000390 GPa
@Strain 5.0 %
0.0566 ksi
@Strain 5.0 %
 0.000710 GPa
@Strain 10 %
0.103 ksi
@Strain 10 %
 0.00140 GPa
@Strain 20 %
0.203 ksi
@Strain 20 %
 0.00174 GPa
@Strain 25 %
0.252 ksi
@Strain 25 %
Compression Set 6.43 %
@Temperature 175 °C,
Time 79200 sec
6.43 %
@Temperature 347 °F,
Time 22.0 hour
ASTM D395
 
Descriptive Properties
ColorOrange

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PAVICON9A8 / 130901

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.