MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Vicone High Performance Rubber VicoSil™ KC605Q-OR High Performance Silicone Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE); Silicone; Silicone Rubber

Material Notes: Anti-fungal grade 1 (GB/T 2423.16-2008). RoHS Approved.

Information provided by Vicone

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.166 g/ccASTM D3165
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 54ASTM D2240
 59.0
@Treatment Temp. 200 °C,
Time 252000 sec
Heat Aging; ASTM D573
Tensile Strength, Yield 8.00 MPaASTM D412
 6.30 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
Heat Aging; ASTM D573
Elongation at Break 551.6 %ASTM D412
 346 %
@Treatment Temp. 200 °C,
Time 252000 sec
Heat Aging; ASTM D573
Compressive Modulus 0.390 MPa
@Strain 5.0 %
 0.710 MPa
@Strain 10 %
 1.40 MPa
@Strain 20 %
 1.74 MPa
@Strain 25 %
Compression Set 6.43 %
@Temperature 175 °C,
Time 79200 sec
ASTM D395
 
Descriptive Properties
ColorOrange

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PAVICON9A8 / 130901

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.