MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 332.0-T5, Permanent Mold Cast
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 332.0-T5; UNS A03320; AA332.0-T5; Al332.0-T5
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.76 g/cc0.0997 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 90 - 12090 - 120AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 132132Estimated from Brinell Hardness.
Hardness, Rockwell A 4242Estimated from Brinell Hardness.
Hardness, Rockwell B 6666Estimated from Brinell Hardness.
Hardness, Vickers 118118Estimated from Brinell Hardness.
Tensile Strength, Ultimate >= 214 MPa>= 31000 psiAA
Tensile Strength, Yield 193 MPa
@Strain 0.2 %
28000 psi
@Strain 0.2 %
Elongation at Break 1.0 %1.0 %in 50 mm
Tensile Modulus 73.0 GPa10600 ksiEstimated from 360.0
Poissons Ratio 0.330.33Estimated from 360.0
Machinability 30 %30 %0-100 Scale (100=best)
Shear Modulus 27.4 GPa3970 ksiCalculated
Shear Strength 131 MPa19000 psiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000660 ohm-cm0.00000660 ohm-cmAA; Typical 26% IACS Conductivity
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 389 J/g167 BTU/lbTypical for cast aluminum
CTE, linear  20.7 µm/m-°C
@Temperature 20.0 - 100 °C
11.5 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical
 22.3 µm/m-°C
@Temperature 20.0 - 300 °C
12.4 µin/in-°F
@Temperature 68.0 - 572 °F
AA; Typical; average over range
Specific Heat Capacity 0.963 J/g-°C0.230 BTU/lb-°FTypical for cast aluminum
Thermal Conductivity 105 W/m-K725 BTU-in/hr-ft²-°FAA; Typical at 25°C
Melting Point 521 - 582 °C970 - 1080 °FAA; Typical
Solidus 521 °C970 °FAA; Typical
Liquidus 582 °C1080 °FAA; Typical
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 80.1 - 88.7 %80.1 - 88.7 %As remainder
Copper, Cu 2.0 - 4.0 %2.0 - 4.0 %
Iron, Fe <= 1.2 %<= 1.2 %
Magnesium, Mg 0.50 - 1.5 %0.50 - 1.5 %
Manganese, Mn <= 0.50 %<= 0.50 %
Nickel, Ni <= 0.50 %<= 0.50 %
Other, total <= 0.50 %<= 0.50 %
Silicon, Si 8.8 - 10.5 %8.8 - 10.5 %
Titanium, Ti <= 0.25 %<= 0.25 %
Zinc, Zn <= 1.0 %<= 1.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum A356.0-T61, Permanent Mold Cast
Aluminum 413.0-F Die Casting Alloy
Aluminum 336.0-T551, Permanent Mold Cast
Aluminum 319.0-T6, Permanent Mold Cast
Aluminum A319.0 Composition Spec

MAC3320T5 / 9875

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.