MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Celanese Hytrel® DYM350BK TPC-ET+PBT
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: Medium Modulus Polyester Elastomer with Excellent Impact Resistance Developed for Air Bag Door Applications

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.18 g/ccISO 1183
Melt Density 1.00 g/cc
@Temperature 245 °C
Water Absorption 0.60 %
@Time 86400 sec
Immersion; Sim. to ISO 62
 0.60 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.014 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.015 cm/cmISO 294-4, 2577
Melt Flow 14 g/10 min
@Load 2.16 kg,
Temperature 240 °C
cm³/10min Volumetric; ISO 1133
 15 g/10 min
@Load 2.16 kg,
Temperature 240 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Puncture Resistance 3200 N
@Temperature 23.0 °C
maximum force; ISO 6603-2
Hardness, Shore D 5015s; ISO 48-4
 <= 55ISO 48-4
Tensile Stress at Strain 10.5 MPa
@Strain 5.0 %
1BA specimen at 50mm/min; ISO 527-1/-2
 13.0 MPa
@Strain 10 %
ISO 527-1/-2
 16.0 MPa
@Strain 50 %
ISO 527-1/-2
Flexural Modulus 430 MPaISO 178
Charpy Impact Unnotched NB
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Puncture Energy 39.0 J
@Temperature 23.0 °C
ISO 6603-2
Tear Strength 105 kN/mnormal; ISO 34-1
 130 kN/mparallel; ISO 34-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 62631-3-1
Surface Resistance 5.00e+14 ohmIEC 62631-3-2
Dielectric Constant 4.4
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.6
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 20.0 kV/mmIEC 60243-1
Dissipation Factor 0.0070
@Frequency 100 Hz
IEC 62631-2-1
 0.023
@Frequency 1e+6 Hz
IEC 62631-2-1
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 180 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 180 µm/m-°CISO 11359-1/-2
Melting Point 222 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 50.0 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 40.0 °CISO 75-1/-2
Brittleness Temperature -100 °CISO 974
Glass Transition Temp, Tg -55.0 °C10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
IEC 60695-11-10
 HB
@Thickness 3.00 mm
IEC 60695-11-10
Flame Spread 23.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
Oxygen Index 22 %ISO 4589-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 245 °COptimum, Injection
 240 - 250 °CRange, Injection
Mold Temperature 45.0 °COptimum, Injection
 40.0 - 55.0 °CInjection
Drying Temperature 100 °CInjection
Dry Time 3.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.050 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)5.44E-08
Emission of organic compounds (µgC/g)2.7VDA 277
FMVSS ClassSE/BISO 3795 (FMVSS 302)
Odor Class5VDA 270
Polymer(TPC+PBT)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Hytrel® DYM250S BK472 TPC-ET+PBT
Celanese Hytrel® 5526 TPC-ET
Celanese Hytrel® HTR8068 TPC-ET-FR(17)
Celanese Hytrel® HTR8223 BK320 TPC-ET
Celanese Hytrel® HTR8341C BK320 TPC-ET

PDSX5195 / 197835

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.