MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Thermal Ceramics Pyro-Bloc R Y and Y2 Modules
Categories: Ceramic; Oxide; Silicon Oxide

Material Notes: The Pyro-Bloc Y and Y2 modules are manufactured from a high purity blend of raw materials which are used to produce R Grade (alumina-silica) ceramic fibers. The modules utilize a specially designed 316 stainless steel internal support system and industry standard Pyro-Bloc stud system. In addition, it has no hot face, cold face, or side constrictions which permit maximum module-to-module compression during installation. The modules use the proven center-fire, one-step weld system which eliminates the need for pre-laid out stud patterns.

Features:

  • Monolithic, edge-grained ceramic fiber module
  • Available in uncompressed densities from 8 - 15 pcf (128-240 kg/m3 )
  • One-shot center-fired stud
  • Extremely fast, efficient installation
  • High density fiber resists mechanical abuse
  • Applications:

  • Annealing furnaces
  • Heat treating furnaces
  • Process heaters
  • Reformers
  • Ethylene furnaces
  • Forge furnaces
  • Steam flood units
  • Homogenizing furnaces
  • Incinerators
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.128 g/cc0.00462 lb/in³Available in multiple densities
     0.160 g/cc0.00578 lb/in³Available in multiple densities
     0.192 g/cc0.00694 lb/in³Available in multiple densities
     0.240 g/cc0.00867 lb/in³Available in multiple densities
    Thickness 3000 - 12000 microns118 - 472 mil
     
    Thermal PropertiesMetricEnglishComments
    Thermal Conductivity  0.0706 W/m-K
    @Temperature 260 °C
    0.490 BTU-in/hr-ft²-°F
    @Temperature 500 °F
    15 pcf; ASTM C201
     0.0720 W/m-K
    @Temperature 260 °C
    0.500 BTU-in/hr-ft²-°F
    @Temperature 500 °F
    12 pcf; ASTM C201
     0.0749 W/m-K
    @Temperature 260 °C
    0.520 BTU-in/hr-ft²-°F
    @Temperature 500 °F
    10 pcf; ASTM C201
     0.0764 W/m-K
    @Temperature 260 °C
    0.530 BTU-in/hr-ft²-°F
    @Temperature 500 °F
    8 pcf; ASTM C201
     0.121 W/m-K
    @Temperature 538 °C
    0.840 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
    15 pcf; ASTM C201
     0.138 W/m-K
    @Temperature 538 °C
    0.960 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
    12 pcf; ASTM C201
     0.150 W/m-K
    @Temperature 538 °C
    1.04 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
    10 pcf; ASTM C201
     0.163 W/m-K
    @Temperature 538 °C
    1.13 BTU-in/hr-ft²-°F
    @Temperature 1000 °F
    8 pcf; ASTM C201
     0.206 W/m-K
    @Temperature 816 °C
    1.43 BTU-in/hr-ft²-°F
    @Temperature 1500 °F
    15 pcf; ASTM C201
     0.239 W/m-K
    @Temperature 816 °C
    1.66 BTU-in/hr-ft²-°F
    @Temperature 1500 °F
    12 pcf; ASTM C201
     0.261 W/m-K
    @Temperature 816 °C
    1.81 BTU-in/hr-ft²-°F
    @Temperature 1500 °F
    10 pcf; ASTM C201
     0.284 W/m-K
    @Temperature 816 °C
    1.97 BTU-in/hr-ft²-°F
    @Temperature 1500 °F
    8 pcf; ASTM C201
     0.316 W/m-K
    @Temperature 1090 °C
    2.19 BTU-in/hr-ft²-°F
    @Temperature 2000 °F
    15 pcf; ASTM C201
     0.353 W/m-K
    @Temperature 1090 °C
    2.45 BTU-in/hr-ft²-°F
    @Temperature 2000 °F
    12 pcf; ASTM C201
     0.388 W/m-K
    @Temperature 1090 °C
    2.69 BTU-in/hr-ft²-°F
    @Temperature 2000 °F
    10 pcf; ASTM C201
     0.425 W/m-K
    @Temperature 1090 °C
    2.95 BTU-in/hr-ft²-°F
    @Temperature 2000 °F
    8 pcf; ASTM C201
    Maximum Service Temperature, Air 1200 °C2200 °FContinuous
     1320 °C2400 °FRating
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 47 %47 %
    SiO2 53 %53 %
     
    Descriptive Properties
    Loss on Ignition trace
    Other Element Contenttraces

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Morgan Advanced Ceramics Kaowool HP Veneering Module Thermal Ceramic
    Morgan Advanced Ceramics Kaowool Ceramic Felt 1260 Thermal Ceramic
    Morgan Advanced Ceramics Kaowool C Veneering Module Thermal Ceramic
    Morgan Advanced Ceramics Green Glass Paper Thermal Ceramic
    Morgan Advanced Ceramics Ceramic Fiber Papers STD Paper Ceramic Fiber

    CTHERM094 / 2414

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.