MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Kaiser 7068 T6, T6511 Rod & Bar
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: Alloy 7068 offers some of the highest strength mechanical properties available in an extruded product. Intended for aerospace, ordnance and light weight recreational applications where extremely high strength is required. Property levels are typically in the 100 ksi range for ultimate strengths.

  • Ratings A through E are relative ratings in decreasing order of merit, based on exposures to sodium chloride solution by intermittent spraying or immersion. Alloys with A and B ratings can be used in industrial and seacoast atmospheres without protection. Alloys with C, D and E ratings generally should be protected at least on faying surfaces.
  • Stress-corrosion cracking ratings are based on service experience and laboratory tests of specimens exposed to the 3.5% sodium chloride alternate immersion test.
    A= No known instance of failure in service or in laboratory tests.
    B= No known instance of failure in service; limited failures in laboratory tests of short transverse specimens.
    C= Service failures with sustained tension stress acting in short transverse direction relative to grain structure; limited failures in laboratory tests of long transverse specimens.
    D= Limited service failures with sustained longitudinal or long transverse
  • Ratings A through D for Workability (cold), A through E for Machinability and A through C for Anodize Response, are relative ratings in decreasing order of merit.
  • Ratings A through D for Weldability and Brazeability are relative ratings defined as follows:
    A= Generally weldable by all commercial procedures and methods.
    B= Weldable with special techniques or for specific applications that justify preliminary trials or testing to develop welding procedure and weld performance.
    C= Limited weldability because of crack sensitivity or loss in resistance to corrosion and mechanical properties.
    D= No commonly used welding methods have been developed.

AMS 4331

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.85 g/cc0.103 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 190
@Load 500 kg,
Thickness 10.0 mm
190
@Load 1100 lb,
Thickness 0.394 in
Tensile Strength, Ultimate 710 MPa
@Diameter 12.7 mm
103000 psi
@Diameter 0.500 in
Tensile Strength, Yield 683 MPa
@Diameter 12.7 mm
99100 psi
@Diameter 0.500 in
Elongation at Break 9.0 %
@Diameter 12.7 mm
9.0 %
@Diameter 0.500 in
4D
Fracture Toughness 16.482 MPa-m½15.000 ksi-in½T-L
 27.471 MPa-m½25.000 ksi-in½L-T
Shear Strength 365 MPa52900 psiUltimate
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000494 ohm-cm
@Temperature 20.0 °C
0.00000494 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 23.4 µm/m-°C
@Temperature 20.0 - 100 °C
13.0 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 1.05 J/g-°C
@Temperature 100 °C
0.250 BTU/lb-°F
@Temperature 212 °F
Thermal Conductivity 190 W/m-K
@Temperature 20.0 °C
1320 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 476 - 635 °C889 - 1180 °F
Solidus 476 °C889 °F
Liquidus 635 °C1180 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 85.48 - 88.85 %85.48 - 88.85 %As Balance
Chromium, Cr <= 0.050 %<= 0.050 %
Copper, Cu 1.6 - 2.4 %1.6 - 2.4 %
Iron, Fe <= 0.15 %<= 0.15 %
Magnesium, Mg 2.2 - 3.0 %2.2 - 3.0 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.050 %<= 0.050 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.12 %<= 0.12 %
Titanium, Ti <= 0.10 %<= 0.10 %
Zinc, Zn 7.3 - 8.3 %7.3 - 8.3 %
Zirconium, Zr 0.050 - 0.15 %0.050 - 0.15 %
 
Descriptive Properties
Anodize Response3B
Arc Weldability4D
Brazeability4D
Cold Workability3D
Gas Weldability4D
General Corrosion Resistance1C
Machinability3C
Spot Weldability4B
Stress Corrosion Resistance2C
Volumetric CTE m³/m³-K0.00006868°F/20°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 7068-T6; 7068-T651 Rod & Bar
Alcoa 7055-T77511 Aluminum Extrusions
Kaiser 7068 T6, T651 Rod & Bar
Aluminum 7068-T6; 7068-T6511 Rod & Bar
Aluminum 7475-T7651

NKAISER0 / 17660

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.