MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
410 Stainless Steel, tempered at 650°C
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes: 16 mm diameter bar, heated to 980°C for 30 min., oil quenched, 650°C temper for 2 hours, air cooled

Key Words: AFNOR Z 12 C 13, UNI X 12 Cr 13, JIS SUS 410, SS14 2302 (Sweden), B.S. 410 S 21, UNS S41000, AMS 5504, AMS 5505, AMS 5591, AMS 5613, AMS 5776, AMS 5821, ASME SA194 (6), ASME SA240, ASME SA268, ASME SA479, ASTM A176, ASTM A193, ASTM A194, ASTM A240, ASTM A276, ASTM A314, ASTM A473, ASTM A479, ASTM A493, ASTM A511, martensitic, ASTM A580, FED QQ-S-763, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405 (51410), B.S. En. 56 A, B.S. ANC 1 Grade A (U.K), SAE J412 (51410), DIN 1.4006, AFNOR Z 10 C 13, AFNOR Z 10 C 14 (France), ISO 683/13 3
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.80 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 274Converted from Rockwell C hardness
Hardness, Rockwell C 24.5before testing
Hardness, Vickers 266Converted from Rockwell C hardness
Tensile Strength, Ultimate 834 MPa
 305 MPa
@Temperature 650 °C
 405 MPa
@Temperature 595 °C
 495 MPa
@Temperature 540 °C
 585 MPa
@Temperature 480 °C
 635 MPa
@Temperature 425 °C
 696 MPa
@Temperature 315 °C
 741 MPa
@Temperature 205 °C
Tensile Strength, Yield 721 MPa
@Strain 0.2 %
 280 MPa
@Strain 0.2 %,
Temperature 650 °C
 385 MPa
@Strain 0.2 %,
Temperature 595 °C
 470 MPa
@Strain 0.2 %,
Temperature 540 °C
 525 MPa
@Strain 0.2 %,
Temperature 480 °C
 570 MPa
@Strain 0.2 %,
Temperature 425 °C
 615 MPa
@Strain 0.2 %,
Temperature 315 °C
 650 MPa
@Strain 0.2 %,
Temperature 205 °C
Elongation at Break 21.5 %in 50 mm
 16 %
@Temperature 315 °C
in 50 mm
 17 %
@Temperature 425 °C
in 50 mm
 18 %
@Temperature 205 °C
in 50 mm
 18.5 %
@Temperature 480 °C
in 50 mm
 22.5 %
@Temperature 540 °C
in 50 mm
 25.5 %
@Temperature 595 °C
in 50 mm
 29 %
@Temperature 650 °C
in 50 mm
Reduction of Area 68.5 %
 68 %
@Temperature 425 °C
 69 %
@Temperature 205 °C
 70 %
@Temperature 315 °C
 73.5 %
@Temperature 480 °C
 81.5 %
@Temperature 540 °C
 88 %
@Temperature 595 °C
 90 %
@Temperature 650 °C
Modulus of Elasticity 200 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000570 ohm-cm
@Temperature 20.0 °C
 0.000108 ohm-cm
@Temperature 650 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.90 µm/m-°C
@Temperature 0.000 - 100 °C
 11.0 µm/m-°C
@Temperature 0.000 - 315 °C
 11.5 µm/m-°C
@Temperature 0.000 - 540 °C
 11.7 µm/m-°C
@Temperature 0.000 - 650 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
Thermal Conductivity 24.9 W/m-K
@Temperature 100 °C
 28.7 W/m-K
@Temperature 500 °C
Melting Point 1480 - 1530 °C
Solidus 1480 °C
Liquidus 1530 °C
Maximum Service Temperature, Air 705 °CContinuous Service
 815 °CIntermittent
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Chromium, Cr 11.5 - 13.5 %
Iron, Fe 84.3 - 88.5 %as balance
Manganese, Mn <= 1.0 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
410 Stainless Steel, tempered at 233°C
410 Stainless Steel, tempered at 343°C
410 Stainless Steel
410 Stainless Steel, tempered at 453°C
410 Stainless Steel, tempered at 678°C

MQ410AJ / 12958

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.