MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Pressure Seal 3717 Nitrile - Butadiene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 3717 is a 70 durometer black colored Buna N elastomer, it is formulated with molybdenum disulfide to provide self lubrication. It exhibits good resistance to aromatic and aliphatic fuels.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 BF 715 B14 B34 EO14; 2 BG 715 B14 B34 EA14 EF11 EF21 EO14; 5 BG 715 A14 B14 B34 EO14
This Compound is RoHS Compliant

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.39 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 74
 60
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 63
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 72
@Treatment Temp. 100 °C,
Time 252000 sec
Distilled water aged
 74
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 79
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 81
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 81
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 83
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 86
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 86
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 86
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 88
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 88
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 88
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
Tensile Strength 1648 psi
 1349.7 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1397.5 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 1626.58 psi
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 1739.4 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 1804.6 psi
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 1854.4 psi
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1895.2 psi
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 1944.6 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 2056.7 psi
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 2086.4 psi
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
 2101.2 psi
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 2181.95 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 2181.95 psi
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 431 %
 234.9 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged
 234.9 %
@Treatment Temp. 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 246.96 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #3
 277.13 %
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #3
 309.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 309.9 %
@Treatment Temp. 100 °C,
Time 252000 sec
Heat Aged
 343.1 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1
 361.2 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel B
 368.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 383.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3
 421.1 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 546.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
ASTM Oil #1
 661.2 %
@Treatment Temp. 150 °C,
Time 252000 sec
ASTM Oil #1
100% Modulus 547 psi
Tear Strength 249 pliDie C
 315 pliDie B
Compression Set 8.1 %
@Treatment Temp. 100 °C,
Time 79200 sec
Solid
 10.7 %
@Treatment Temp. 125 °C,
Time 79200 sec
Solid
 12.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
Solid
 22.2 %
@Treatment Temp. 100 °C,
Time 79200 sec
Plied
 23 %
@Treatment Temp. 125 °C,
Time 79200 sec
Plied
 23.5 %
@Treatment Temp. 100 °C,
Time 252000 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -17.0 °F
Shrinkage -9.30 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -7.30 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -6.60 %
@Treatment Temp. 125 °C,
Time 252000 sec
Volume, ASTM Oil #1
 -0.600 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 -0.400 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, ASTM Oil #3
 0.90 %
@Treatment Temp. 125 °C,
Time 252000 sec
Volume, ASTM Oil #3
 1.2 %
@Treatment Temp. 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 7.7 %
@Treatment Temp. 100 °C,
Time 252000 sec
Volume, Distilled water aged
 15.9 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel B
 26.6 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL015 / 318225

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.