MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.27 - 1.76 g/ccAverage value: 1.57 g/cc Grade Count:232
 1.31 - 1.49 g/cc
@Temperature 223 - 250 °C
Average value: 1.41 g/cc Grade Count:6
Filler Content 5.00 - 32.0 %Average value: 22.7 % Grade Count:73
Water Absorption 0.000 - 4.00 %Average value: 0.194 % Grade Count:108
Moisture Absorption at Equilibrium 0.0500 - 0.500 %Average value: 0.199 % Grade Count:59
Water Absorption at Saturation 0.150 - 0.500 %Average value: 0.332 % Grade Count:15
Viscosity 150 - 3.50e+6 cP
@Temperature 230 - 270 °C
Average value: 934000 cP Grade Count:2
 150 - 3.50e+6 cP
@Shear Rate 1.00 - 100000 1/s
Average value: 934000 cP Grade Count:2
Viscosity Number 62.0 - 112 cm³/gAverage value: 96.0 cm³/g Grade Count:10
Maximum Moisture Content 0.0200Average value: 0.0200 Grade Count:8
Linear Mold Shrinkage 0.000500 - 0.0200 cm/cmAverage value: 0.00571 cm/cm Grade Count:159
 0.00300 - 0.00400 cm/cm
@Temperature 260 - 260 °C
Average value: 0.00333 cm/cm Grade Count:3
 0.00300 - 0.00400 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.00333 cm/cm Grade Count:3
Linear Mold Shrinkage, Transverse 0.00100 - 0.0180 cm/cmAverage value: 0.0102 cm/cm Grade Count:57
 0.0110 - 0.0130 cm/cm
@Temperature 260 - 260 °C
Average value: 0.0120 cm/cm Grade Count:3
 0.0110 - 0.0130 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.0120 cm/cm Grade Count:3
Melt Flow 1.00 - 75.0 g/10 minAverage value: 17.0 g/10 min Grade Count:77
Ash 0.0350 - 30.0 %Average value: 7.53 % Grade Count:8
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 70.0 - 100Average value: 92.8 Grade Count:17
Hardness, Rockwell R 90.0 - 120Average value: 116 Grade Count:28
Ball Indentation Hardness 160 - 235 MPaAverage value: 199 MPa Grade Count:4
Tensile Strength, Ultimate 15.0 - 154 MPaAverage value: 108 MPa Grade Count:195
Tensile Strength, Yield 68.0 - 150 MPaAverage value: 106 MPa Grade Count:44
Elongation at Break 0.900 - 50.0 %Average value: 3.34 % Grade Count:201
Elongation at Yield 2.50 - 9.00 %Average value: 4.33 % Grade Count:6
Modulus of Elasticity 0.765 - 21.2 GPaAverage value: 8.54 GPa Grade Count:104
Flexural Yield Strength 70.3 - 230 MPaAverage value: 162 MPa Grade Count:163
Flexural Modulus 1.86 - 11.3 GPaAverage value: 7.01 GPa Grade Count:165
Flexural Strain at Break 3.00 - 3.50 %Average value: 3.23 % Grade Count:3
Flexural Strain at Yield 2.20 - 4.90 %Average value: 3.02 % Grade Count:15
Poissons Ratio 0.330 - 0.350Average value: 0.341 Grade Count:14
Izod Impact, Notched 0.267 - 4.27 J/cmAverage value: 0.709 J/cm Grade Count:100
 0.300 - 0.450 J/cm
@Temperature -20.0 - -20.0 °C
Average value: 0.375 J/cm Grade Count:2
Izod Impact, Unnotched 0.490 - 9.61 J/cmAverage value: 5.18 J/cm Grade Count:13
Izod Impact, Notched (ISO) 3.00 - 10.0 kJ/m²Average value: 8.64 kJ/m² Grade Count:32
 7.00 - 10.0 kJ/m²
@Temperature -30.0 - -30.0 °C
Average value: 9.67 kJ/m² Grade Count:15
Izod Impact, Unnotched (ISO) 20.0 - 55.0 kJ/m²Average value: 41.7 kJ/m² Grade Count:18
 20.0 - 55.0 kJ/m²
@Temperature -30.0 - -30.0 °C
Average value: 39.8 kJ/m² Grade Count:16
Charpy Impact Unnotched 2.30 - 8.00 J/cm²Average value: 4.39 J/cm² Grade Count:86
 1.20 - 7.50 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 4.18 J/cm² Grade Count:48
Charpy Impact, Notched 0.230 - 2.00 J/cm²Average value: 0.761 J/cm² Grade Count:124
 0.180 J/cm² - NB
@Temperature -40.0 - -20.0 °C
Average value: 0.731 J/cm² Grade Count:51
Tensile Impact Strength 8.00 - 55.0 kJ/m²Average value: 37.7 kJ/m² Grade Count:3
Tensile Creep Modulus, 1 hour 5000 - 11000 MPaAverage value: 7580 MPa Grade Count:4
Tensile Creep Modulus, 1000 hours 3000 - 8000 MPaAverage value: 5780 MPa Grade Count:4
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1000 - 1.00e+18 ohm-cmAverage value: 2.08e+16 ohm-cm Grade Count:120
Surface Resistance 1000 - 1.00e+17 ohmAverage value: 9.11e+15 ohm Grade Count:52
Dielectric Constant 3.00 - 4.50Average value: 3.55 Grade Count:65
Dielectric Strength 16.0 - 44.0 kV/mmAverage value: 25.3 kV/mm Grade Count:84
Dissipation Factor 0.00100 - 0.0220Average value: 0.0110 Grade Count:45
Arc Resistance 60.0 - 120 secAverage value: 104 sec Grade Count:14
Comparative Tracking Index 125 - 600 VAverage value: 291 V Grade Count:83
Hot Wire Ignition, HWI 7.00 - 120 secAverage value: 70.9 sec Grade Count:6
High Amp Arc Ignition, HAI 30.0 - 120 arcsAverage value: 113 arcs Grade Count:5
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.0 - 67.0 µm/m-°CAverage value: 35.3 µm/m-°C Grade Count:96
 16.0 - 20.0 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 19.0 µm/m-°C Grade Count:4
CTE, linear, Transverse to Flow 50.0 - 120 µm/m-°CAverage value: 81.8 µm/m-°C Grade Count:52
 140 - 140 µm/m-°C
@Temperature 55.0 - 160 °C
Average value: 140 µm/m-°C Grade Count:1
Specific Heat Capacity 1.60 - 1.60 J/g-°C
@Temperature 250 - 250 °C
Average value: 1.60 J/g-°C Grade Count:1
Thermal Conductivity 0.173 - 0.202 W/m-KAverage value: 0.180 W/m-K Grade Count:4
 0.260 - 0.260 W/m-K
@Temperature 250 - 250 °C
Average value: 0.260 W/m-K Grade Count:1
Melting Point 200 - 250 °CAverage value: 224 °C Grade Count:93
Maximum Service Temperature, Air 90.0 - 215 °CAverage value: 153 °C Grade Count:7
Hot Ball Pressure Test 165 - 220 °CAverage value: 206 °C Grade Count:8
Deflection Temperature at 0.46 MPa (66 psi) 138 - 225 °CAverage value: 212 °C Grade Count:135
Deflection Temperature at 1.8 MPa (264 psi) 70.0 - 250 °CAverage value: 199 °C Grade Count:202
Deflection Temperature at 8.0 MPa 65.0 - 165 °CAverage value: 123 °C Grade Count:3
Vicat Softening Point 165 - 225 °CAverage value: 207 °C Grade Count:43
Glass Transition Temp, Tg 55.0 °CAverage value: 55.0 °C Grade Count:12
UL RTI, Electrical 75.0 - 140 °CAverage value: 117 °C Grade Count:11
UL RTI, Mechanical with Impact 75.0 - 140 °CAverage value: 117 °C Grade Count:11
UL RTI, Mechanical without Impact 75.0 - 140 °CAverage value: 112 °C Grade Count:11
Flammability, UL94 HB - 5VAGrade Count:219
Oxygen Index 28.0 - 40.0 %Average value: 33.1 % Grade Count:11
Glow Wire Test 675 - 960 °CAverage value: 891 °C Grade Count:63
 
Processing PropertiesOriginal ValueComments
Processing Temperature 204 - 270 °CAverage value: 251 °C Grade Count:26
Nozzle Temperature 225 - 270 °CAverage value: 250 °C Grade Count:25
Melt Temperature 220 - 280 °CAverage value: 249 °C Grade Count:95
Mold Temperature 30.0 - 130 °CAverage value: 78.9 °C Grade Count:108
Drying Temperature 80.0 - 140 °CAverage value: 117 °C Grade Count:82
Moisture Content 0.000 - 0.300 %Average value: 0.0586 % Grade Count:38
Dew Point -40.0 - -28.9 °CAverage value: -37.2 °C Grade Count:4
Injection Pressure 4.96 - 120 MPaAverage value: 81.2 MPa Grade Count:25
Vent Depth 0.00127 - 0.00381 cmAverage value: 0.00196 cm Grade Count:11

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), Flame Retardant
Overview of materials for Polybutylene Terephthalate (PBT), Glass Bead Filled
Overview of materials for Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

O3210 / 78170

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.