MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polybutylene Terephthalate (PBT), Glass Bead Filled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Glass Bead Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), Glass Bead Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.25 - 1.73 g/cc0.0452 - 0.0625 lb/in³Average value: 1.52 g/cc Grade Count:67
Filler Content 10.0 - 40.0 %10.0 - 40.0 %Average value: 26.4 % Grade Count:11
Water Absorption 0.0500 - 0.500 %0.0500 - 0.500 %Average value: 0.158 % Grade Count:30
Moisture Absorption at Equilibrium 0.100 - 0.250 %0.100 - 0.250 %Average value: 0.166 % Grade Count:20
Water Absorption at Saturation 0.310 - 0.500 %0.310 - 0.500 %Average value: 0.395 % Grade Count:11
Viscosity  18.0 - 700000 cP
@Temperature 230 - 270 °C
18.0 - 700000 cP
@Temperature 446 - 518 °F
Average value: 104000 cP Grade Count:4
 18.0 - 700000 cP
@Shear Rate 1.00 - 100000 1/s
18.0 - 700000 cP
@Shear Rate 1.00 - 100000 1/s
Average value: 104000 cP Grade Count:4
Maximum Moisture Content  0.200 - 0.200
@Temperature 120 - 120 °C
0.200 - 0.200
@Temperature 248 - 248 °F
Average value: 0.200 Grade Count:2
 0.200 - 0.200
@Time 299 - 299 sec
0.200 - 0.200
@Time 0.0830 - 0.0830 hour
Average value: 0.200 Grade Count:2
Linear Mold Shrinkage 0.00200 - 0.0250 cm/cm0.00200 - 0.0250 in/inAverage value: 0.0123 cm/cm Grade Count:46
 0.0140 - 0.0160 cm/cm
@Temperature 260 - 260 °C
0.0140 - 0.0160 in/in
@Temperature 500 - 500 °F
Average value: 0.0150 cm/cm Grade Count:2
 0.0140 - 0.0160 cm/cm
@Pressure 60.0 - 60.0 MPa
0.0140 - 0.0160 in/in
@Pressure 8700 - 8700 psi
Average value: 0.0150 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00200 - 0.0250 cm/cm0.00200 - 0.0250 in/inAverage value: 0.0144 cm/cm Grade Count:18
 0.0140 - 0.0160 cm/cm
@Temperature 260 - 260 °C
0.0140 - 0.0160 in/in
@Temperature 500 - 500 °F
Average value: 0.0150 cm/cm Grade Count:2
 0.0140 - 0.0160 cm/cm
@Pressure 60.0 - 60.0 MPa
0.0140 - 0.0160 in/in
@Pressure 8700 - 8700 psi
Average value: 0.0150 cm/cm Grade Count:2
Melt Flow 4.00 - 48.0 g/10 min4.00 - 48.0 g/10 minAverage value: 23.2 g/10 min Grade Count:20
Ash 18.0 - 30.0 %
@Temperature 625 - 625 °C
18.0 - 30.0 %
@Temperature 1160 - 1160 °F
Average value: 25.3 % Grade Count:2
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 65.0 - 95.065.0 - 95.0Average value: 80.0 Grade Count:4
Hardness, Rockwell R 117 - 120117 - 120Average value: 118 Grade Count:11
Ball Indentation Hardness 150 - 200 MPa21800 - 29000 psiAverage value: 170 MPa Grade Count:6
Tensile Strength, Ultimate 40.7 - 155 MPa5900 - 22500 psiAverage value: 69.0 MPa Grade Count:55
Tensile Strength, Yield 44.1 - 120 MPa6400 - 17400 psiAverage value: 55.6 MPa Grade Count:14
Elongation at Break 1.80 - 16.0 %1.80 - 16.0 %Average value: 3.83 % Grade Count:65
Elongation at Yield 2.80 - 4.00 %2.80 - 4.00 %Average value: 3.15 % Grade Count:4
Modulus of Elasticity 2.75 - 15.2 GPa399 - 2200 ksiAverage value: 5.52 GPa Grade Count:47
Flexural Yield Strength 77.9 - 245 MPa11300 - 35500 psiAverage value: 115 MPa Grade Count:41
Flexural Modulus 2.10 - 13.1 GPa305 - 1900 ksiAverage value: 4.74 GPa Grade Count:41
Compressive Yield Strength 49.6 - 138 MPa7200 - 20000 psiAverage value: 73.8 MPa Grade Count:8
Izod Impact, Notched 0.267 - 12.0 J/cm0.500 - 22.5 ft-lb/inAverage value: 0.988 J/cm Grade Count:30
Izod Impact, Unnotched 2.40 - 6.41 J/cm4.50 - 12.0 ft-lb/inAverage value: 3.89 J/cm Grade Count:18
Izod Impact, Notched (ISO) 3.50 - 13.0 kJ/m²1.67 - 6.19 ft-lb/in²Average value: 6.67 kJ/m² Grade Count:9
 3.00 - 12.0 kJ/m²
@Temperature -30.0 - -30.0 °C
1.43 - 5.71 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 7.33 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) 15.3 - 80.0 kJ/m²7.28 - 38.1 ft-lb/in²Average value: 38.7 kJ/m² Grade Count:6
 20.0 - 190 kJ/m²
@Temperature -30.0 - -30.0 °C
9.52 - 90.4 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 66.3 kJ/m² Grade Count:4
Charpy Impact Unnotched 2.20 - 8.50 J/cm²10.5 - 40.5 ft-lb/in²Average value: 3.95 J/cm² Grade Count:27
 1.90 - 6.50 J/cm²
@Temperature -30.0 - -20.0 °C
9.04 - 30.9 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 3.46 J/cm² Grade Count:18
Charpy Impact, Notched 0.170 - 1.30 J/cm²0.809 - 6.19 ft-lb/in²Average value: 0.494 J/cm² Grade Count:35
 0.200 - 1.30 J/cm²
@Temperature -30.0 - -20.0 °C
0.952 - 6.19 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 0.602 J/cm² Grade Count:16
Tensile Creep Modulus, 1000 hours 1300 - 2700 MPa189000 - 392000 psiAverage value: 2070 MPa Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+6 - 1.00e+18 ohm-cm1.00e+6 - 1.00e+18 ohm-cmAverage value: 3.09e+16 ohm-cm Grade Count:42
Surface Resistance 3.00 - 1.00e+17 ohm3.00 - 1.00e+17 ohmAverage value: 9.77e+15 ohm Grade Count:22
Dielectric Constant 2.60 - 4.502.60 - 4.50Average value: 3.79 Grade Count:24
Dielectric Strength 15.0 - 100 kV/mm381 - 2540 kV/inAverage value: 27.4 kV/mm Grade Count:32
Dissipation Factor 0.00120 - 0.1300.00120 - 0.130Average value: 0.0193 Grade Count:16
Arc Resistance 110 - 150 sec110 - 150 secAverage value: 133 sec Grade Count:9
Comparative Tracking Index 125 - 500 V125 - 500 VAverage value: 291 V Grade Count:19
 
Thermal PropertiesMetricEnglishComments
CTE, linear 21.6 - 110 µm/m-°C12.0 - 61.1 µin/in-°FAverage value: 66.0 µm/m-°C Grade Count:33
 140 - 140 µm/m-°C
@Temperature 60.0 - 138 °C
77.8 - 77.8 µin/in-°F
@Temperature 140 - 280 °F
Average value: 140 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 68.0 - 130 µm/m-°C37.8 - 72.2 µin/in-°FAverage value: 89.7 µm/m-°C Grade Count:17
 150 - 150 µm/m-°C
@Temperature 60.0 - 138 °C
83.3 - 83.3 µin/in-°F
@Temperature 140 - 280 °F
Average value: 150 µm/m-°C Grade Count:1
Thermal Conductivity 0.159 - 0.270 W/m-K1.10 - 1.87 BTU-in/hr-ft²-°FAverage value: 0.207 W/m-K Grade Count:10
Melting Point 200 - 228 °C392 - 442 °FAverage value: 224 °C Grade Count:31
Maximum Service Temperature, Air 120 - 200 °C248 - 392 °FAverage value: 151 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 80.0 - 220 °C176 - 428 °FAverage value: 191 °C Grade Count:43
Deflection Temperature at 1.8 MPa (264 psi) 62.8 - 213 °C145 - 415 °FAverage value: 138 °C Grade Count:61
Vicat Softening Point 180 - 245 °C356 - 473 °FAverage value: 200 °C Grade Count:13
Flammability, UL94 HB - V-0HB - V-0Grade Count:47
Oxygen Index 21.0 - 23.0 %21.0 - 23.0 %Average value: 22.3 % Grade Count:3
Glow Wire Test 650 - 750 °C1200 - 1380 °FAverage value: 717 °C Grade Count:9
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 271 °C68.0 - 520 °FAverage value: 207 °C Grade Count:20
Nozzle Temperature 249 - 277 °C480 - 530 °FAverage value: 260 °C Grade Count:3
Melt Temperature 220 - 280 °C428 - 536 °FAverage value: 252 °C Grade Count:27
Mold Temperature 26.7 - 110 °C80.0 - 230 °FAverage value: 78.2 °C Grade Count:42
Drying Temperature 80.0 - 130 °C176 - 266 °FAverage value: 115 °C Grade Count:28
Moisture Content 0.000 - 0.100 %0.000 - 0.100 %Average value: 0.0453 % Grade Count:15
Injection Pressure 50.0 - 103 MPa7250 - 15000 psiAverage value: 84.1 MPa Grade Count:16

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant
Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), Aramid Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), Carbon Black Filled

O3217 / 78176

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.