MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter No. 883® Hot Work Die Steel (Red-Tough) (AISI H13)
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: No. 883 hot work die steel is a 5% chromium hot work tool steel designed particularly for applications requiring extreme toughness combined with good red-hardness. It has given an extra margin of safety in tools subject to heavy hammer blows, and those tools containing deep recesses or sharp corners. While No. 833 hot work die steel has been used primarily in hot work tools, it has solved many cold work applications where extra toughness was required at the sacrifice of some wear resistance.

Applications: Forging dies, Heavy duty compression tools, Bulldozer dies, Hot forging tools with deep recesses and sharp corners, Die casting dies, Aluminum extrusion dies, Bolt dies, Hot piercing punches, Forming punches, Vastoning dies

Information provided by Carpenter Technology Corporation.

No. 883® is a registered trademark of Carpenter Technology Corporation.

Key Words: UNS T20813
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 7.77 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 360
@Temperature 538 °C
 495
@Temperature 204 °C
Hardness, Rockwell C 28 - 30Tempered at 1300°F
 51 - 53As hardened
Tensile Strength, Ultimate 1800 MPawhen tempered at 1000°F
Tensile Strength, Yield 1600 MPawhen tempered at 1000°F
Elongation at Break 11 %when tempered at 1000°F
Reduction of Area 35 %when tempered at 1000°F
Modulus of Elasticity 210.3 GPa
 113.8 GPa
@Temperature 649 °C
 191 GPa
@Temperature 343 °C
Charpy Impact 22.0 JV Notch, when tempered at 1000°F
Abrasion 128.4loss in mm3, As-Hardened; ASTM G65
 186loss in mm3, Tempered at 1200°F; ASTM G65
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.0 µm/m-°C
@Temperature 27.0 - 93.0 °C
 13.1 µm/m-°C
@Temperature 27.0 - 649 °C
 14.8 µm/m-°C
@Temperature 427 - 788 °C
Specific Heat Capacity 0.110 BTU/lb-°F
Thermal Conductivity 28.6 W/m-K
@Temperature 216 °C
Transformation Temperature 818 °CAc1
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.41 %
Chromium, Cr 5.35 %
Iron, Fe 90.59 %As Balance
Manganese, Mn 0.35 %
Molybdenum, Mo 1.4 %
Silicon, Si 1.0 %
Vanadium, V 0.90 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type H13 Hot Work Tool Steel
Bohler-Uddeholm SUPERIOR® H13 Hot Work Tool Steel
Bohler-Uddeholm UDDEHOLM ORVAR® SUPERIOR (Premium AISI H13) Hot Work Tool Steel
Latrobe LSS™ H13 Tool Steel (ASTM H13)
Bohler-Uddeholm ORVAR® 2M / AISI H13 Hot Work Tool Steel

NCARN22 / 15861

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.