MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Celstran® PA66-GF40-02 40% Long Glass Fiber Reinforced Nylon 6/6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled

Material Notes: Description: 40% long strand glass fiber reinforced heat stabilized Nylon 6/6

Information provided by Celanese Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.45 g/cc0.0524 lb/in³ISO 1183 & ASTM D792
Linear Mold Shrinkage 0.0010 - 0.0020 cm/cm0.0010 - 0.0020 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0020 - 0.0030 cm/cm0.0020 - 0.0030 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 215 MPa31200 psi5 mm/min; ISO 527-2/1A
 253 MPa36700 psiASTM D638
 270 MPa
@Temperature -40.0 °C
39100 psi
@Temperature -40.0 °F
ASTM D638
Tensile Strength, Ultimate 134 MPa
@Temperature 121 °C
19400 psi
@Temperature 250 °F
ASTM D638
Elongation at Break 2.0 %2.0 %5 mm/min; ISO 527-2/1A
 2.3 %2.3 %ASTM D638
 2.2 %
@Temperature -40.0 °C
2.2 %
@Temperature -40.0 °F
ASTM D638
 2.5 %
@Temperature 121 °C
2.5 %
@Temperature 250 °F
ASTM D638
Tensile Modulus 13.3 GPa1930 ksi1 mm/min; ISO 527-2/1A
 14.2 GPa2060 ksiASTM D638
 7.31 GPa
@Temperature 121 °C
1060 ksi
@Temperature 250 °F
ASTM D638
 14.5 GPa
@Temperature -40.0 °C
2100 ksi
@Temperature -40.0 °F
ASTM D638
Flexural Strength 355 MPa51500 psiISO 178
 359 MPa52000 psiASTM D790
 181 MPa
@Temperature 121 °C
26300 psi
@Temperature 250 °F
ASTM D790
 388 MPa
@Temperature -40.0 °C
56300 psi
@Temperature -40.0 °F
ASTM D790
Flexural Modulus 11.8 GPa1710 ksiISO 178
 12.3 GPa1780 ksiASTM D790
 6.48 GPa
@Temperature 121 °C
940 ksi
@Temperature 250 °F
ASTM D790
 12.45 GPa
@Temperature -40.0 °C
1805 ksi
@Temperature -40.0 °F
ASTM D790
Izod Impact, Notched 3.68 J/cm6.90 ft-lb/inASTM D256
 4.64 J/cm8.70 ft-lb/inat 250°F; ASTM D256
 3.95 J/cm
@Temperature -40.0 °C
7.40 ft-lb/in
@Temperature -40.0 °F
ASTM D256
Charpy Impact, Notched 3.50 J/cm²16.7 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 255 °C491 °FISO 75-1, -2 & ASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® B3 GF 40 (2474) PA 6 Dry, 40% Glass Filled
Domo Technyl® A 216 V40 40% Glass Filled Nylon 66
MTI ThermoStran® PA66-30C Long Carbon Fiber Compound
BASF Capron® GR40 40% Glass-Filled Nylon 6 (Conditioned)
Overview of materials for Nylon 66, 40% Glass Fiber Filled

PHCV17 / 45857

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.