MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes 242® alloy, after 8000 hours exposure at 650°C (1200°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Age-hardenable, high ductility in the aged condition, lower thermal expansion than most alloys, very good oxidation resistance up to 815°C, excellent low cycle fatigue properties, very good thermal stability, and resistance to high-temperature fluorine and fluoride environments. Applications include seal rings, containment rings, duct segments, casings, fasteners, rocket nozzles, pumps, hydrofluoric acid vapor containing processes, fluoroelastomer process equipment such as extrusion screws.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 9.05 g/ccat RT
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 257Converted from Vickers hardness
Hardness, Knoop 286Converted from Vickers hardness
Hardness, Rockwell C 19Converted from Vickers hardness
Hardness, Vickers 78
@Temperature 870 °C
 140
@Temperature 760 °C
 218
@Temperature 650 °C
 263
@Temperature 540 °C
 271
@Temperature 425 °C
Tensile Strength, Ultimate 1330 MPa
Tensile Strength, Yield 835 MPa
@Strain 0.2 %
Elongation at Break 24 %in 50 mm
Reduction of Area 24 %
Modulus of Elasticity 229 GPaRT
 152 GPa
@Temperature 1000 °C
 163 GPa
@Temperature 900 °C
 172 GPa
@Temperature 800 °C
 185 GPa
@Temperature 700 °C
 193 GPa
@Temperature 600 °C
 199 GPa
@Temperature 500 °C
 206 GPa
@Temperature 400 °C
 213 GPa
@Temperature 300 °C
 219 GPa
@Temperature 200 °C
 225 GPa
@Temperature 100 °C
Charpy Impact 35.0 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000122 ohm-cmRT
 0.0001234 ohm-cm
@Temperature 100 °C
 0.0001251 ohm-cm
@Temperature 200 °C
 0.0001267 ohm-cm
@Temperature 300 °C
 0.0001276 ohm-cm
@Temperature 1000 °C
 0.000128 ohm-cm
@Temperature 400 °C
 0.0001295 ohm-cm
@Temperature 500 °C
 0.0001298 ohm-cm
@Temperature 900 °C
 0.0001306 ohm-cm
@Temperature 600 °C
 0.000132 ohm-cm
@Temperature 700 °C
 0.0001324 ohm-cm
@Temperature 800 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.8 µm/m-°C
@Temperature 25.0 - 100 °C
 11.3 µm/m-°C
@Temperature 25.0 - 200 °C
 11.6 µm/m-°C
@Temperature 25.0 - 300 °C
 11.9 µm/m-°C
@Temperature 25.0 - 400 °C
 12.2 µm/m-°C
@Temperature 25.0 - 500 °C
 12.3 µm/m-°C
@Temperature 25.0 - 600 °C
 12.4 µm/m-°C
@Temperature 25.0 - 650 °C
 13.0 µm/m-°C
@Temperature 25.0 - 700 °C
 13.7 µm/m-°C
@Temperature 25.0 - 750 °C
 14.0 µm/m-°C
@Temperature 25.0 - 800 °C
 14.5 µm/m-°C
@Temperature 25.0 - 900 °C
 15.0 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.386 J/g-°CRT
 0.405 J/g-°C
@Temperature 100 °C
 0.419 J/g-°C
@Temperature 200 °C
 0.431 J/g-°C
@Temperature 300 °C
 0.439 J/g-°C
@Temperature 400 °C
 0.451 J/g-°C
@Temperature 500 °C
 0.470 J/g-°C
@Temperature 600 °C
 0.595 J/g-°C
@Temperature 700 °C
 0.605 J/g-°C
@Temperature 800 °C
 0.610 J/g-°C
@Temperature 900 °C
 0.627 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 11.3 W/m-KRT
 12.6 W/m-K
@Temperature 100 °C
 14.2 W/m-K
@Temperature 200 °C
 15.9 W/m-K
@Temperature 300 °C
 17.5 W/m-K
@Temperature 400 °C
 19.2 W/m-K
@Temperature 500 °C
 20.9 W/m-K
@Temperature 600 °C
 22.5 W/m-K
@Temperature 700 °C
 24.2 W/m-K
@Temperature 800 °C
 25.8 W/m-K
@Temperature 900 °C
 27.5 W/m-K
@Temperature 1000 °C
Melting Point 1290 - 1375 °C
Solidus 1290 °C
Liquidus 1375 °C
Maximum Service Temperature, Air 815 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al <= 0.50 %
Boron, B <= 0.0060 %
Carbon, C <= 0.030 %
Chromium, Cr 7.0 - 9.0 %
Cobalt, Co <= 2.5 %
Copper, Cu <= 0.50 %
Iron, Fe <= 2.0 %
Manganese, Mn <= 0.80 %
Molybdenum, Mo 24 - 26 %
Nickel, Ni 58 %As Remainder
Silicon, Si <= 0.80 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Rene 85 Nickel Superalloy
ATI Allvac® Rene 41® Nickel Superalloy, Heat Treatment: 1079°C (1975°F) + Age
Haynes 188 alloy, 10% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 0% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 20% cold reduction, 3.2 mm thick sheet

NH24BT / 16553

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.