MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 242® alloy, after 8000 hours exposure at 650°C (1200°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Age-hardenable, high ductility in the aged condition, lower thermal expansion than most alloys, very good oxidation resistance up to 815°C, excellent low cycle fatigue properties, very good thermal stability, and resistance to high-temperature fluorine and fluoride environments. Applications include seal rings, containment rings, duct segments, casings, fasteners, rocket nozzles, pumps, hydrofluoric acid vapor containing processes, fluoroelastomer process equipment such as extrusion screws.

Data provided by the manufacturer, Haynes International, Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 9.05 g/cc0.327 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 257257Converted from Vickers hardness
Hardness, Knoop 286286Converted from Vickers hardness
Hardness, Rockwell C 1919Converted from Vickers hardness
Hardness, Vickers  78
@Temperature 870 °C
78
@Temperature 1600 °F
 140
@Temperature 760 °C
140
@Temperature 1400 °F
 218
@Temperature 650 °C
218
@Temperature 1200 °F
 263
@Temperature 540 °C
263
@Temperature 1000 °F
 271
@Temperature 425 °C
271
@Temperature 797 °F
Tensile Strength, Ultimate 1330 MPa193000 psi
Tensile Strength, Yield 835 MPa
@Strain 0.2 %
121000 psi
@Strain 0.2 %
Elongation at Break 24 %24 %in 50 mm
Reduction of Area 24 %24 %
Modulus of Elasticity 229 GPa33200 ksiRT
 152 GPa
@Temperature 1000 °C
22000 ksi
@Temperature 1830 °F
 163 GPa
@Temperature 900 °C
23600 ksi
@Temperature 1650 °F
 172 GPa
@Temperature 800 °C
24900 ksi
@Temperature 1470 °F
 185 GPa
@Temperature 700 °C
26800 ksi
@Temperature 1290 °F
 193 GPa
@Temperature 600 °C
28000 ksi
@Temperature 1110 °F
 199 GPa
@Temperature 500 °C
28900 ksi
@Temperature 932 °F
 206 GPa
@Temperature 400 °C
29900 ksi
@Temperature 752 °F
 213 GPa
@Temperature 300 °C
30900 ksi
@Temperature 572 °F
 219 GPa
@Temperature 200 °C
31800 ksi
@Temperature 392 °F
 225 GPa
@Temperature 100 °C
32600 ksi
@Temperature 212 °F
Charpy Impact 35.0 J25.8 ft-lb
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000122 ohm-cm0.000122 ohm-cmRT
 0.0001234 ohm-cm
@Temperature 100 °C
0.0001234 ohm-cm
@Temperature 212 °F
 0.0001251 ohm-cm
@Temperature 200 °C
0.0001251 ohm-cm
@Temperature 392 °F
 0.0001267 ohm-cm
@Temperature 300 °C
0.0001267 ohm-cm
@Temperature 572 °F
 0.0001276 ohm-cm
@Temperature 1000 °C
0.0001276 ohm-cm
@Temperature 1830 °F
 0.000128 ohm-cm
@Temperature 400 °C
0.000128 ohm-cm
@Temperature 752 °F
 0.0001295 ohm-cm
@Temperature 500 °C
0.0001295 ohm-cm
@Temperature 932 °F
 0.0001298 ohm-cm
@Temperature 900 °C
0.0001298 ohm-cm
@Temperature 1650 °F
 0.0001306 ohm-cm
@Temperature 600 °C
0.0001306 ohm-cm
@Temperature 1110 °F
 0.000132 ohm-cm
@Temperature 700 °C
0.000132 ohm-cm
@Temperature 1290 °F
 0.0001324 ohm-cm
@Temperature 800 °C
0.0001324 ohm-cm
@Temperature 1470 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.8 µm/m-°C
@Temperature 25.0 - 100 °C
6.00 µin/in-°F
@Temperature 77.0 - 212 °F
 11.3 µm/m-°C
@Temperature 25.0 - 200 °C
6.28 µin/in-°F
@Temperature 77.0 - 392 °F
 11.6 µm/m-°C
@Temperature 25.0 - 300 °C
6.44 µin/in-°F
@Temperature 77.0 - 572 °F
 11.9 µm/m-°C
@Temperature 25.0 - 400 °C
6.61 µin/in-°F
@Temperature 77.0 - 752 °F
 12.2 µm/m-°C
@Temperature 25.0 - 500 °C
6.78 µin/in-°F
@Temperature 77.0 - 932 °F
 12.3 µm/m-°C
@Temperature 25.0 - 600 °C
6.83 µin/in-°F
@Temperature 77.0 - 1110 °F
 12.4 µm/m-°C
@Temperature 25.0 - 650 °C
6.89 µin/in-°F
@Temperature 77.0 - 1200 °F
 13.0 µm/m-°C
@Temperature 25.0 - 700 °C
7.22 µin/in-°F
@Temperature 77.0 - 1290 °F
 13.7 µm/m-°C
@Temperature 25.0 - 750 °C
7.61 µin/in-°F
@Temperature 77.0 - 1380 °F
 14.0 µm/m-°C
@Temperature 25.0 - 800 °C
7.78 µin/in-°F
@Temperature 77.0 - 1470 °F
 14.5 µm/m-°C
@Temperature 25.0 - 900 °C
8.06 µin/in-°F
@Temperature 77.0 - 1650 °F
 15.0 µm/m-°C
@Temperature 25.0 - 1000 °C
8.33 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.386 J/g-°C0.0923 BTU/lb-°FRT
 0.405 J/g-°C
@Temperature 100 °C
0.0968 BTU/lb-°F
@Temperature 212 °F
 0.419 J/g-°C
@Temperature 200 °C
0.100 BTU/lb-°F
@Temperature 392 °F
 0.431 J/g-°C
@Temperature 300 °C
0.103 BTU/lb-°F
@Temperature 572 °F
 0.439 J/g-°C
@Temperature 400 °C
0.105 BTU/lb-°F
@Temperature 752 °F
 0.451 J/g-°C
@Temperature 500 °C
0.108 BTU/lb-°F
@Temperature 932 °F
 0.470 J/g-°C
@Temperature 600 °C
0.112 BTU/lb-°F
@Temperature 1110 °F
 0.595 J/g-°C
@Temperature 700 °C
0.142 BTU/lb-°F
@Temperature 1290 °F
 0.605 J/g-°C
@Temperature 800 °C
0.145 BTU/lb-°F
@Temperature 1470 °F
 0.610 J/g-°C
@Temperature 900 °C
0.146 BTU/lb-°F
@Temperature 1650 °F
 0.627 J/g-°C
@Temperature 1000 °C
0.150 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 11.3 W/m-K78.4 BTU-in/hr-ft²-°FRT
 12.6 W/m-K
@Temperature 100 °C
87.4 BTU-in/hr-ft²-°F
@Temperature 212 °F
 14.2 W/m-K
@Temperature 200 °C
98.5 BTU-in/hr-ft²-°F
@Temperature 392 °F
 15.9 W/m-K
@Temperature 300 °C
110 BTU-in/hr-ft²-°F
@Temperature 572 °F
 17.5 W/m-K
@Temperature 400 °C
121 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.2 W/m-K
@Temperature 500 °C
133 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.9 W/m-K
@Temperature 600 °C
145 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.5 W/m-K
@Temperature 700 °C
156 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.2 W/m-K
@Temperature 800 °C
168 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 25.8 W/m-K
@Temperature 900 °C
179 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 27.5 W/m-K
@Temperature 1000 °C
191 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1290 - 1375 °C2350 - 2507 °F
Solidus 1290 °C2350 °F
Liquidus 1375 °C2507 °F
Maximum Service Temperature, Air 815 °C1500 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.50 %<= 0.50 %
Boron, B <= 0.0060 %<= 0.0060 %
Carbon, C <= 0.030 %<= 0.030 %
Chromium, Cr 7.0 - 9.0 %7.0 - 9.0 %
Cobalt, Co <= 2.5 %<= 2.5 %
Copper, Cu <= 0.50 %<= 0.50 %
Iron, Fe <= 2.0 %<= 2.0 %
Manganese, Mn <= 0.80 %<= 0.80 %
Molybdenum, Mo 24 - 26 %24 - 26 %
Nickel, Ni 58 %58 %As Remainder
Silicon, Si <= 0.80 %<= 0.80 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Rene 85 Nickel Superalloy
ATI Allvac® Rene 41® Nickel Superalloy, Heat Treatment: 1079°C (1975°F) + Age
Haynes 188 alloy, 10% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 0% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 20% cold reduction, 3.2 mm thick sheet

NH24BT / 16553

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.