MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Westlake EF524 14.5% Ethylene Vinyl Acetate Copolymer
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate

Material Notes: Westlake ELEVATE™ EF524 is an ethylene vinyl acetate copolymer with 14.5% VA. EF524 is designed for blown and cast films requiring excellent optics and low heat seal initiation. High melt strength makes EF524 an excellent choice for profile extrusions, molding, and foaming applications requiring high VA content..

    Application/Uses
  • Flexible packaging films
  • Peelable seals, adhesive layers
  • Injection and blow molding
  • Profile extrusions, tubing, wire & cable

This resin grade complies with 21 CFR, section 177.1350.

Key Words: Excellent optics and low heat seal initiation. 14.5% EVA
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.934 g/ccD1505
Vinyl Acetate Content 14.5 %
Thickness 45.7 micronsThickness Tested
Melt Flow 3.5 g/10 minD1238
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 675 %D882
Film Elongation at Break, TD 100 %D882
Dart Drop 8.11 g/micronD1709
Dart Drop Test 370 gD1709
Film Tensile Strength at Break, MD 22.1 MPaD638
Film Tensile Strength at Break, TD 20.7 MPaD638
1% Secant Modulus, MD 50.0 MPaD882
1% Secant Modulus, TD 55.2 MPaD882
 
Thermal PropertiesOriginal ValueComments
Melting Point 90.0 °CDSC Peak; D3418
 
Optical PropertiesOriginal ValueComments
Haze 1.5 %D1003
Gloss 87 %at 45; D2457
 
Processing PropertiesOriginal ValueComments
Melt Temperature 193 °CBlown Film
 210 °CCast Film
Blow-up Ratio (BUR) 2.5
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.
 
Descriptive Properties
processFilm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Braskem PN2021 EVA Foam Copolymer
Westlake ELEVATE™ EF529 18.5% Ethylene Vinyl Acetate Copolymer
Braskem VA2019A EVA Foam Copolymer
Westlake EF528 18.5% Ethylene Vinyl Acetate Copolymer
Arkema Evatane® 1020 VG 5 Ethylene Vinyl Acetate

PBP1130 / 133378

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.