MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Solvay VTM® 264FRB Epoxy Resin
Categories: Polymer; Thermoset; Epoxy

Material Notes: VTM264FRB is a black, flame-retarded, controlled flow epoxy resin matrices systems with a broad 65 to 120°C (150 to 250°F) processing window, offering low temperate initial cures or reduced total cycle times. VTM264FRB and VTM267FRB are formatted for a range of low cost, vacuum-bag pressure, composite molding processes, including ZPREG partial impregnation technology. VTM267FRB offers enhanced workshop handling characteristics with and controlled tack for sided impregnation and film infusion processing with heavy reinforcements.

Features & Benefits:

  • Open vacuum bag curing
  • 21 days out life 21°C (70°F)
  • 12 months storage at -18°C (0°F)
  • Self-extinguishing to FMVSS30/ISO3795/SAE J369
  • Flexible cure between 65 at 120°C (149 and 248°F)
  • Minimum initial cure temperature 65°C (149°F)
  • Maximum dry service temperature of 100°C (212°F) following suitable post-cure
  • Excellent tack and drape for easy lay-up of large structures, vertical surfaces and complex shapes
  • VTM267FRB offers controlled tack for sided impregnation and film infusion processing
  • Compatible with all VTM260 and ZPREG260 series materials
Note 1: Cure cycle: 1 hr at 120°C (248°F), 6.2 bar (90 psi)

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0441 lb/in³1 hr at 120°C
Storage Temperature -18.0 °C-0.400 °F
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 100 °C212 °Fdry
Glass Transition Temp, Tg 83.0 °C181 °FDMA E' 16 hrs at 65°C
 100 °C212 °FDMA E' 5 hrs at 80°C
 120 °C248 °FDMA E' 2 hrs at 100°C
 120 °C248 °FDMA E' 1 hr at 120°C
 125 °C257 °FDMA E' 16 hrs at 65°C+1 hr at 120°C
 
Processing PropertiesMetricEnglishComments
Shelf Life 12.0 Month12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay CYCOM® 977-2 Neat Epoxy Resin
SGL Carbon Group SIGRAFIL C® C30 T045 EPY Continuous Tow Carbon Fiber with 45k filaments, Epoxy Sizing
Nanocyl PREGCYL™ NC R2HM-01 Pre-impregnated UD/Fabric Carbon Fibers
Huntsman Araldite PY 302-2 Bisphenol F Epoxy Resin
Huntsman Araldite 98-311 Bisphenol F Epoxy Resin

PCYTED168 / 180470

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.