MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Sandvik SAF 2304 Seamless tube and pipe
Categories: Metal; Ferrous Metal; Duplex; Stainless Steel

Material Notes: Duplex stainless steel, UNS S32304

Sandvik SAF 2304TM is a duplex stainless steel (austenitic-ferritic) with a low carbon content. The material is characterized by the following properties:

  • very good resistance to stress corrosion cracking.
  • good resistance to general corrosion an pitting.
  • high strength - approximately twice as high proof strength as austenitic stainless steels.
  • physical properties that offer design advantages.
  • ease of fabrication and good toughness.
  • good weldability
  • Information provided by Sandvik

    UNS S32304; EN 1.4362

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 7.80 g/cc0.282 lb/in³
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Rockwell C <= 30.5<= 30.5
    Tensile Strength, Ultimate 600 - 820 MPa87000 - 119000 psi
    Tensile Strength, Yield  >= 400 MPa
    @Strain 0.2 %
    >= 58000 psi
    @Strain 0.2 %
     >= 450 MPa
    @Strain 1 %
    >= 65300 psi
    @Strain 1 %
     >= 270 MPa
    @Strain 0.2 %,
    Temperature 300 °C
    >= 39200 psi
    @Strain 0.2 %,
    Temperature 572 °F
    Wt>4 mm
     >= 290 MPa
    @Strain 0.2 %,
    Temperature 200 °C
    >= 42100 psi
    @Strain 0.2 %,
    Temperature 392 °F
    Wt>4 mm
     >= 310 MPa
    @Strain 0.2 %,
    Temperature 300 °C
    >= 45000 psi
    @Strain 0.2 %,
    Temperature 572 °F
    Wt<4 mm
     >= 340 MPa
    @Strain 0.2 %,
    Temperature 200 °C
    >= 49300 psi
    @Strain 0.2 %,
    Temperature 392 °F
    Wt<4 mm
    Elongation at Break >= 25 %>= 25 %
     >= 25 %
    @Thickness 50.8 mm
    >= 25 %
    @Thickness 2.00 in
    Modulus of Elasticity 200 GPa29000 ksi
     180 GPa
    @Temperature 300 °C
    26100 ksi
    @Temperature 572 °F
     186 GPa
    @Temperature 200 °C
    27000 ksi
    @Temperature 392 °F
    Charpy Impact  175 J
    @Temperature -50.0 °C
    129 ft-lb
    @Temperature -58.0 °F
    welded
     275 J
    @Temperature -50.0 °C
    203 ft-lb
    @Temperature -58.0 °F
    unwelded
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear  13.5 µm/m-°C
    @Temperature 30.0 - 100 °C
    7.50 µin/in-°F
    @Temperature 86.0 - 212 °F
     14.0 µm/m-°C
    @Temperature 30.0 - 200 °C
    7.78 µin/in-°F
    @Temperature 86.0 - 392 °F
     14.5 µm/m-°C
    @Temperature 30.0 - 400 °C
    8.06 µin/in-°F
    @Temperature 86.0 - 752 °F
    Specific Heat Capacity  0.490 J/g-°C
    @Temperature 20.0 °C
    0.117 BTU/lb-°F
    @Temperature 68.0 °F
     0.530 J/g-°C
    @Temperature 200 °C
    0.127 BTU/lb-°F
    @Temperature 392 °F
     0.590 J/g-°C
    @Temperature 400 °C
    0.141 BTU/lb-°F
    @Temperature 752 °F
    Thermal Conductivity  16.0 W/m-K
    @Temperature 20.0 °C
    111 BTU-in/hr-ft²-°F
    @Temperature 68.0 °F
     17.0 W/m-K
    @Temperature 200 °C
    118 BTU-in/hr-ft²-°F
    @Temperature 392 °F
     21.0 W/m-K
    @Temperature 400 °C
    146 BTU-in/hr-ft²-°F
    @Temperature 752 °F
     
    Component Elements PropertiesMetricEnglishComments
    Carbon, C <= 0.030 %<= 0.030 %
    Chromium, Cr 22.5 %22.5 %
    Iron, Fe 69.8 %69.8 %As Balance
    Manganese, Mn <= 2.0 %<= 2.0 %
    Nickel, Ni 4.5 %4.5 %
    Nitrogen, N 0.10 %0.10 %
    Phosphorus, P <= 0.035 %<= 0.035 %
    Silicon, Si <= 1.0 %<= 1.0 %
    Sulfur, S <= 0.015 %<= 0.015 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Sandvik SAF 2205 Seamless tube and pipe
    304 Stainless Steel
    Sandvik SAF 2507 Seamless tube and pipe
    Sandvik SAF 2304 Plate, Sheet and Coil
    AISI Type 304L Stainless Steel

    NSANDV247 / 19141

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.