MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Thermal Ceramics Therm-O-Seal Finishing Cements
Categories: Ceramic

Material Notes: Therm-O-Seal Finishing Cement is a general purpose, hydraulic setting cement, with excellent troweling, and palming properties. It has extremely low drying shrinkage, and hardens to a smooth crack-free surface within a few hours. Once dry, Therm-O-Seal Finishing Cement is highly resistant to weather damage, but water-based paint may be applied to improve appearance.

Therm-O-Seal Finishing Cement provides a strong protective coating for other insulating materials. Used as a finish over insulation cement, brick, or other block insulation, Therm-OSeal creates a very tight seal which further reduces cold air infiltration and heat loss.

Features:

  • Finishing cement recommended for temperatures up to 1400°F
  • Finishing cement provides a strong protective coating for other insulation materials
  • Insulating cement recommended for temperatures up to 1800°F
  • Insulating cement is a non-corrosive cement with outstanding adhesion
  • Fibrous adhesive maximum service temperature 1200°F
  • No asbestos fibers
  • Fast setting compound
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 0.200 g/cc0.00723 lb/in³dry
     0.481 g/cc0.0174 lb/in³wet
    Loss On Ignition 4.5 %4.5 %
     
    Mechanical PropertiesMetricEnglishComments
    Compressive Yield Strength 0.138 MPa20.1 psi5% deformation
     
    Thermal PropertiesMetricEnglishComments
    Thermal Conductivity  0.110 W/m-K
    @Temperature 204 °C
    0.760 BTU-in/hr-ft²-°F
    @Temperature 400 °F
    ASTM C201
     0.140 W/m-K
    @Temperature 427 °C
    0.970 BTU-in/hr-ft²-°F
    @Temperature 800 °F
    ASTM C201
     0.180 W/m-K
    @Temperature 649 °C
    1.25 BTU-in/hr-ft²-°F
    @Temperature 1200 °F
    ASTM C201
     0.225 W/m-K
    @Temperature 871 °C
    1.56 BTU-in/hr-ft²-°F
    @Temperature 1600 °F
    ASTM C201
    Maximum Service Temperature, Air 760 °C1400 °F
     
    Component Elements PropertiesMetricEnglishComments
    Al2O3 16 %16 %
    Alkalis 6.9 %6.9 %
    CaO 2.7 %2.7 %
    Fe2O3 7.3 %7.3 %
    MgO 18 %18 %
    SiO2 44 %44 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    CTHERM255 / 2575

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.