MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

E-Polymers SEPAZ® K365GM 60% Glass Fiber/Calcium Carbonate Reinforced General Purpose PPS Resin
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: Polyphenylene Sulfide Resin: High-performance engineering plastic SEPAZ PPS boasts excellent high-temperature resistance, flame retardancy and chemical resistance, physical strength, and its fluidity leads to good dimensional precision. SEPAZ PPS applications: switches, connectors and other electronic and electric components, alternators and other automobile components, and office equipment components including chassis parts and housings.

Information Provided by E-Polymers Co., Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.96 g/cc1.96 g/ccASTM D792
Water Absorption 0.020 %
@Time 86400 sec
0.020 %
@Time 24.0 hour
Linear Mold Shrinkage 0.0010 - 0.0020 cm/cm0.0010 - 0.0020 in/in
Linear Mold Shrinkage, Transverse 0.0030 - 0.0050 cm/cm0.0030 - 0.0050 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 131.5 MPa19070 psiASTM D638
Elongation at Break 1.0 %1.0 %ASTM D638
Flexural Strength 189.33 MPa27460 psiASTM D790
Flexural Modulus 18.84 GPa2732 ksiASTM D790
Izod Impact, Notched 0.422 J/cm0.790 ft-lb/inASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmASTM D257
Dielectric Constant 4.1
@Frequency 1e+6 Hz
4.1
@Frequency 1e+6 Hz
ASTM D150
Dissipation Factor 0.010
@Frequency 1e+6 Hz
0.010
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 µm/m-°C
@Thickness 1.60 mm
10.0 µin/in-°F
@Thickness 0.0630 in
ASTM D696
CTE, linear, Transverse to Flow 31.0 µm/m-°C
@Thickness 1.60 mm
17.2 µin/in-°F
@Thickness 0.0630 in
ASTM D696
Melting Point 280 °C536 °FASTM D789
Deflection Temperature at 1.8 MPa (264 psi) 266 °C511 °FASTM D648
Flammability, UL94 V-0V-0
 
Processing PropertiesMetricEnglishComments
Melt Temperature 300 - 330 °C572 - 626 °F
Mold Temperature 130 - 160 °C266 - 320 °F
Drying Temperature 140 °C284 °F
Dry Time 6 hour6 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
M. Holland Company MTEGRITY™ PP100 Polypropylene Homopolymer, General Purpose
LyondellBasell Pro-fax 6523 Polypropylene Homopolymer, General Purpose
Lotte Advanced Materials Infino® AR-9301 PA, Glass Filled General Purpose
Evonik Vestodur® GF50 nf PBT
Chevron Phillips Xtel® XE3035BL Polyphenylene Sulfide Alloy

PEPOLZ060 / 103557

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.