MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
LyondellBasell Hostalen GD 4755 High Density Polyethylene (HDPE), Injection Molded
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Injection Molded

Material Notes: Exceptional organoleptic properties and a good balance of stiffness, toughness and environmental stress cracking resistance make Hostalen GD4755 the choice of customers for the production of closures for sparkling water, CSD and many other types of food and nonfood caps and closures. Customers also use this material for engineering parts. Applications: Caps & Closures

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.953 g/ccISO 1183-1
Melt Flow 1.9 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133-1
 6.0 g/10 min
@Load 5.00 kg,
Temperature 190 °C
ISO 1133-1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 62ISO 868
Ball Indentation Hardness 51.0 MPaISO 2039-1
Tensile Strength, Yield 27.0 MPaISO 527-1,-2
Elongation at Yield 10 %ISO 527-1,-2
Tensile Modulus 1100 MPaISO 527-1,-2
Charpy Impact, Notched 4.50 kJ/m²
@Temperature -30.0 °C
ISO 179
 6.00 kJ/m²
@Temperature 23.0 °C
ISO 179
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 75.0 °CB50; ISO 306
 
Descriptive Properties
FNCT (hrs)8ISO 16770, 6.0 MPa, 2% Arkopal N100, 50°C
Processing Methodcompression molding, injection molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Hostalen ACP 5331H High Density Polyethylene (HDPE), Injection Molded
LyondellBasell Hostalen ACP 6541A UV High Density Polyethylene (HDPE), Injection Molded
LyondellBasell Hostalen GC 7258 High Density Polyethylene (HDPE), Injection Molded
LyondellBasell Hostalen GC 7260 LS High Density Polyethylene (HDPE), Injection Molded
Braskem GF4950HS HDPE Blow Molding Polyethylene Copolymer

PEQT8481 / 220116

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.