MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Dow Surlyn® 8528 Sodium Ionomer
Categories: Polymer; Thermoplastic; Ionomer

Material Notes: Surlyn® 8528 is a sodium ionomer thermoplastic resin. It is available for use in conventional extrusion and injection equipment, to create various sheets or shapes. Surlyn® 8528 thermoplastic resin is an advanced ethylene/methacrylic acid (E/MAA) copolymer, in which the MAA acid groups have been partially neutralized with sodium ions.

SURLYN® 8528 complies with Food and Drug Administration Regulation 21 CFR 177.1330(a) - - Ionomeric resins, subject to the limitations and requirements therein. This Regulation describes polymers that may be used in contact with food, subject to the finished food-contact article meeting the extractive limitations under the intended conditions of use, as shown in paragraph (c) of the Regulation.

This former DuPont product line is now a Dow product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.940 g/ccASTM D792, ISO 1183
Melt Flow 1.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238, ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 60ASTM D2240, ISO 868
Abrasive Hardness 600NBS Index, ASTM D1630
Tensile Strength at Break 29.0 MPa
@Temperature 23.0 °C
ASTM D638, ISO 527-2
Elongation at Break 450 %
@Temperature 23.0 °C
ASTM D638, ISO 527-2
Flexural Modulus 220 MPa
@Temperature 23.0 °C
ASTM D790
 576 MPa
@Temperature -20.0 °C
ASTM D790
Tensile Impact Strength 445 ft-lb/in²
@Temperature -40.0 °C
ASTM D1822
 550 ft-lb/in²
@Temperature 23.0 °C
ASTM D1822
 
Thermal PropertiesOriginal ValueComments
Melting Point 66.0 °CFreezing Point; ASTM D3418, ISO 3146
 93.0 °CASTM D3418, ISO 3146
Vicat Softening Point 73.0 °CASTM D1525, ISO 306
Brittleness Temperature -95.0 °CASTM D746
 
Optical PropertiesOriginal ValueComments
Haze 6.0 %
@Thickness 6.35 mm
ASTM D1003
 
Processing PropertiesOriginal ValueComments
Processing Temperature <= 285 °C
Melt Temperature 185 - 285 °C
 
Compliance PropertiesOriginal ValueComments
FDA YesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow Surlyn® 1707 Sodium Ionomer
Dow Surlyn® 9320 Zinc Ionomer
Dow Surlyn® 7930 Ionomer Resin, Lithium
Dow Surlyn® 2601B Sodium Ionomer
Dow Surlyn® 6320 Magnesium Ionomer

PDTA4977 / 170417

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.