MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Domo TECHNYL® A 246M PA66, DRY
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Description: Unreinforced and modified polyamide 66, with very high impact resistance even at low temperature, for injection molding.

Available in: Europe and North America

Product Applications: TECHNYL® A 246M offers an excellent notched impact resistance at low temperature make it suitable for: sports and leisure applications, for shoe soles, ski components, ski and surf bindings, toy applications, such as, the bumper of a remote-controlled car. This product is available in natural, white and black.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.08 g/ccISO 1183/A
Water Absorption 1.05 %
@Temperature 23.0 °C,
Time 86400 sec
ISO 62
Linear Mold Shrinkage 0.010 cm/cmIsotropy
Linear Mold Shrinkage, Flow 0.019 cm/cm
Linear Mold Shrinkage, Transverse 0.019 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 44.0 MPaISO 527 Type 1A
Tensile Strength, Yield 47.0 MPaISO 527 type 1 A
 50.0 MPaASTM D638
Tensile Modulus 1900 MPaISO 527 Type 1A
Flexural Strength 70.0 MPaISO 178
Flexural Modulus 1800 MPaISO 178
Izod Impact, Notched (ISO) 22.0 kJ/m²
@Temperature -30.0 °C
ISO 180/1eA
 60.0 kJ/m²
@Temperature 23.0 °C
ISO 180/1eA
Charpy Impact Unnotched 16.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 NB
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 91.0 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 3.2IEC 60250
Dielectric Strength 30.0 kV/mmIEC 60243
Dissipation Factor 0.020IEC 60250
Comparative Tracking Index 450 VSolution B; IEC 60112
 575 VSolution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 23.0 - 85.0 °C
ISO 11359
Melting Point 263 °CISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 200 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °CISO 75/Af
Flammability, UL94 HB
@Thickness 1.60 mm
1210
Oxygen Index 24.5 %ISO 4589
 
Processing PropertiesOriginal ValueComments
Feed Temperature 250 - 270 °C
Mold Temperature 60.0 - 80.0 °C
Drying Temperature 80.0 °C
Moisture Content <= 0.20 %
 
Descriptive Properties
Compression Zone260-280°C
Mixing Zone270-290°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LyondellBasell Hifax TYC007P BLK Thermoplastic Olefinic Elastomer, mineral Filled
Borealis Daplen™ EF210AE Polypropylene TPO Compound
Borealis Daplen™ EF209AE Polypropylene TPO Compound
Domo Technyl® A 246M Nylon 66, Impact Grade, EH0
Borealis Daplen™ EE255AE Polypropylene TPO Compound

PRHOD699 / 137930

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.