MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Pressure Seal 13644 Butyl
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 13644 is a 60 durometer black colored Butyl elastomer, it is formulated with FDA sanctioned materials. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 615 A13 EA14 F17; 3 AA 615 B13 B33 EA14 F17; 4 AA 615 A13 B13 B33 EA14 F17; 5 AA 615 A13 B13 B33 EA14 F17; 2 BA 615 F17; 3 BA 615 A14 B13 F17; 4 BA 615 A14 F17; 5 BA 615 F17

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.09 g/cc1.09 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6060
 58
@Treatment Temp. 100 °C,
Time 252000 sec
58
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 60
@Treatment Temp. 70.0 °C,
Time 252000 sec
60
@Treatment Temp. 158 °F,
Time 70.0 hour
Heat Aged
 62
@Treatment Temp. 100 °C,
Time 252000 sec
62
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
Tensile Strength 13.11 MPa1902 psi
 13.297 MPa
@Treatment Temp. 70.0 °C,
Time 252000 sec
1928.6 psi
@Treatment Temp. 158 °F,
Time 70.0 hour
Heat Aged
 13.966 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
2025.6 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
Elongation, Ultimate 500 %500 %
 460 %
@Treatment Temp. 100 °C,
Time 252000 sec
460 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Heat Aged
 480 %
@Treatment Temp. 70.0 °C,
Time 252000 sec
480 %
@Treatment Temp. 158 °F,
Time 70.0 hour
Heat Aged
100% Modulus 1.17 MPa169 psi
Tear Strength 23.0 kN/m131 pliDie C
 29.3 kN/m167 pliDie B
Compression Set  10.8 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
10.8 %
@Treatment Temp. 158 °F,
Time 22.0 hour
Solid
 12.6 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
12.6 %
@Treatment Temp. 158 °F,
Time 22.0 hour
Plied
 31.3 %
@Treatment Temp. 100 °C,
Time 79200 sec
31.3 %
@Treatment Temp. 212 °F,
Time 22.0 hour
Solid
 46 %
@Treatment Temp. 100 °C,
Time 79200 sec
46 %
@Treatment Temp. 212 °F,
Time 22.0 hour
Plied
 52 %
@Treatment Temp. 100 °C,
Time 252000 sec
52 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Solid
 63.7 %
@Treatment Temp. 100 °C,
Time 252000 sec
63.7 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Plied
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -47.8 °C-54.0 °F
Shrinkage 0.40 %
@Treatment Temp. 100 °C,
Time 252000 sec
0.40 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, Distilled water aged
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL238 / 318448

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.