MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Constellium Certal® Thick Aluminum Plate
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: Certal® thick plates have been optimized to provide excellent machinability, shape stability and high strength. Certal® is therefore ideal for industrial tools. Applications include injection and blow-moulds for plastic bottles, containers, shoes as well as heating plates, guides, tooling supports, jigs and fixtures.

Information provided by manufacturer

Key Words: EN AW-7022; AlZn5Mg3Cu
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.76 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 165
@Thickness 25.0 - 100 mm
 165
@Thickness 100 - 140 mm
 170
@Thickness 7.90 - 25.0 mm
Tensile Strength >= 490 MPa
@Thickness 100 - 140 mm
Temper T651
 >= 500 MPa
@Thickness 50.0 - 100 mm
Temper T651
 >= 530 MPa
@Thickness 25.0 - 50.0 mm
Temper T651
 >= 540 MPa
@Thickness 7.90 - 12.5 mm
Temper T651
 >= 540 MPa
@Thickness 12.5 - 25.0 mm
Temper T651
 545 MPa
@Thickness 100 - 140 mm
Typical Strength
 550 MPa
@Thickness 25.0 - 100 mm
Typical Strength
 555 MPa
@Thickness 7.90 - 25.0 mm
Typical Strength
Tensile Strength, Yield >= 400 MPa
@Strain 0.2 %,
Thickness 100 - 140 mm
Temper T651
 >= 420 MPa
@Strain 0.2 %,
Thickness 50.0 - 100 mm
Temper T651
 >= 460 MPa
@Strain 0.2 %,
Thickness 7.90 - 12.5 mm
Temper T651
 >= 460 MPa
@Strain 0.2 %,
Thickness 12.5 - 25.0 mm
Temper T651
 >= 460 MPa
@Strain 0.2 %,
Thickness 25.0 - 50.0 mm
Temper T651
 490 MPa
@Strain 0.2 %,
Thickness 100 - 140 mm
Typical Strength
 495 MPa
@Strain 0.2 %,
Thickness 7.90 - 25.0 mm
Typical Strength
 495 MPa
@Strain 0.2 %,
Thickness 25.0 - 100 mm
Typical Strength
Elongation at Break >= 6.0 %
@Thickness 50.0 - 100 mm
Temper T651
 >= 6.0 %
@Thickness 100 - 140 mm
Temper T651
 >= 7.0 %
@Thickness 25.0 - 50.0 mm
Temper T651
 7.0 %
@Thickness 100 - 140 mm
Typical Elongation
 8.0 %
@Thickness 25.0 - 100 mm
Typical Elongation
 >= 8.0 %
@Thickness 7.90 - 12.5 mm
Temper T651
 >= 8.0 %
@Thickness 12.5 - 25.0 mm
Temper T651
 9.0 %
@Thickness 7.90 - 25.0 mm
Typical Elongation
Modulus of Elasticity 72.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000450 - 0.00000550 ohm-cmTemper T651
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
Thermal Conductivity 120 - 150 W/m-KTemper T651
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 88.2 - 92.4 %as balance
Chromium, Cr 0.10 - 0.30 %
Copper, Cu 0.50 - 1.0 %
Iron, Fe <= 0.50 %
Magnesium, Mg 2.6 - 3.7 %
Manganese, Mn 0.10 - 0.40 %
Silicon, Si <= 0.50 %
Zinc, Zn 4.3 - 5.2 %
Zr+Ti <= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
7022 Aluminum Composition Spec
7020-T6 Aluminum
Sandvik Osprey CE17 Al-Si Controlled Expansion Alloy
Saint-Gobain Meldin® 7022 DF Direct Formed Graphite Filled Polyimide
Aleris Hokotol Aluminum Alloy, 100 mm Thickness

NCONS016 / 160279

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.