System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Budd DSM-949, Diesel Grade SMC, Vinyl Ester, Black
(discontinued **)
Categories:
Polymer
;
Thermoset
;
Composite SMC
;
Vinyl Ester
;
Vinyl Ester Sheet Molding Compound
Material Notes:
Used for parts requiring high strength at room temperature, good retention of properties at high temperatures and corrosion resistance, such as diesel engine external body parts.
Data provided by the manufacturer.
Key Words:
Polyester Sheet Molding Compound
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.70
g/cc
Water Absorption
<= 0.35 %
ASTM D570-63
Linear Mold Shrinkage
0.00050
cm/cm
Mechanical Properties
Original Value
Comments
Hardness, Barcol
55 - 65
ASTM D2583
Tensile Strength, Ultimate
75.0
-
105
MPa
ASTM D638-68
Flexural Yield Strength
190
MPa
ASTM D790-70
Flexural Modulus
9.70
-
12.4
GPa
ASTM D790-70
Izod Impact, Notched
8.50
J/cm
ASTM D256-70
Thermal Properties
Original Value
Comments
CTE, linear
17.5
µm/m-°C
@Temperature 23.0 - 150 °C
Deflection Temperature at 1.8 MPa (264 psi)
>=
235
°C
ASTM D648-61
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
A. Schulman Premi-Glas® 1266 (Injection Compression Molded) Glass Reinforced TMC
Ensinger TECATOR™ TI 5013 Polyamide-imide (PAI)
Chesterton ARC NVE SYSTEM Vinyl Ester Lining
Hybrid Plastics POSS® MA0702 MethacrylIsobutyl-POSS®
Multibase TPSiV® 3111-70A Thermoplastic Silicone Vulcanizate
PPTB00 / 58259
Free Trade Publications, Click Here!
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.