MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Kennametal Stellite Stellite® 6 PM cast
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Adhesive wear test data: 0.49 P/M, 0.48 Cast; Typical applications include: (aerospace) vane plugs, fuel metering pins, spacer bushings, (bearings) ball blanks, race blanks, (valve seat inserts) diesel engine exhaust, fluid valve seats, saw cutter inserts, miscellaneous wear parts. Data provide by the manufacturer, Deloro Stellite Inc.

Product of former Deloro Stellite Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.20 g/ccP/M (98%)
 8.38 g/cctheoretical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 364Converted from Rockwell C hardness.
 224
@Temperature 760 °C
Converted from Rockwell C hardness
 312
@Temperature 649 °C
Converted from Rockwell C hardness
 345
@Temperature 538 °C
Converted from Rockwell C hardness
Hardness, Knoop 436Converted from Rockwell C hardness.
 262
@Temperature 760 °C
Converted from Rockwell C hardness
 372
@Temperature 649 °C
Converted from Rockwell C hardness
 413
@Temperature 538 °C
Converted from Rockwell C hardness
Hardness, Rockwell A 70Converted from Rockwell C hardness.
 60
@Temperature 760 °C
Converted from Rockwell C hardness
 67
@Temperature 649 °C
Converted from Rockwell C hardness
 69
@Temperature 538 °C
Converted from Rockwell C hardness
Hardness, Rockwell C 40
 19
@Temperature 760 °C
 34
@Temperature 649 °C
 38
@Temperature 538 °C
Hardness, Vickers 383Converted from Rockwell C hardness.
 230
@Temperature 760 °C
Converted from Rockwell C hardness
 326
@Temperature 649 °C
Converted from Rockwell C hardness
 362
@Temperature 538 °C
Converted from Rockwell C hardness
Tensile Strength, Ultimate 911 MPa
 552 MPa
@Temperature 760 °C
 676 MPa
@Temperature 649 °C
 759 MPa
@Temperature 538 °C
Elongation at Break <= 1.0 %in 25.4 mm
 1.0 %
@Temperature 538 °C
in 25.4 mm
 2.0 %
@Temperature 649 °C
in 25.4 mm
 5.0 %
@Temperature 760 °C
in 25.4 mm
 
Electrical PropertiesOriginal ValueComments
Magnetic Permeability <= 1.2
@Temperature 22.0 °C
200 Oersted
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.9 µm/m-°C
@Temperature 0.000 - 100 °C
 14.1 µm/m-°C
@Temperature 0.000 - 200 °C
 14.5 µm/m-°C
@Temperature 0.000 - 300 °C
 14.7 µm/m-°C
@Temperature 0.000 - 400 °C
 15.0 µm/m-°C
@Temperature 0.000 - 500 °C
 15.3 µm/m-°C
@Temperature 0.000 - 600 °C
 15.8 µm/m-°C
@Temperature 0.000 - 700 °C
 16.3 µm/m-°C
@Temperature 0.000 - 800 °C
 16.9 µm/m-°C
@Temperature 0.000 - 900 °C
 17.4 µm/m-°C
@Temperature 0.000 - 1000 °C
Melting Point 1260 - 1357 °C
Solidus 1260 °C
Liquidus 1357 °C
 
Component Elements PropertiesOriginal ValueComments
Boron, B <= 1.0 %
Carbon, C 1.2 %
Chromium, Cr 29 %
Cobalt, Co 52.3 %As remainder
Iron, Fe <= 3.0 %
Manganese, Mn 1.0 %
Molybdenum, Mo <= 1.5 %
Nickel, Ni <= 3.0 %
Other <= 2.0 %
Silicon, Si <= 1.5 %
Tungsten, W 4.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kennametal Stellite Stellite® 6 PM with P/M Processing
Kennametal Stellite Stoody® 6 Cobalt-Base Cast Alloy
Kennametal Stellite Stellite® 3 PM with P/M Processing
Kennametal Stellite Stellite® 12
Kennametal Stellite Stellite® 4 Cobalt Chromium Alloy

NS6PMB / 18881

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.