MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Multibase Nylex™ 4032 Polyamide + PP
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Polypropylene (PP)

Material Notes:

Forms:

  • Pellets
  • Information provided by Multibase

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.15 g/cc1.15 g/ccASTM 792
    Linear Mold Shrinkage 0.0040 cm/cm0.0040 in/inASTM D955
    Melt Flow 1.5 g/10 min
    @Load 2.16 kg,
    Temperature 230 °C
    1.5 g/10 min
    @Load 4.76 lb,
    Temperature 446 °F
    ASTM D1238
     
    Mechanical PropertiesMetricEnglishComments
    Tensile Strength, Ultimate 48.3 MPa7000 psiASTM D638
    Elongation at Break 20 %20 %ASTM D638
    Flexural Strength 62.1 MPa9000 psiASTM D790
    Flexural Modulus 3.45 GPa500 ksiMethod I (3 point load), Procedure B); ASTM D790
    Izod Impact, Notched 1.07 J/cm2.00 ft-lb/in73°F; ASTM D256
    Gardner Impact 2.825 J2.083 ft-lbASTM D3029
     
    Thermal PropertiesMetricEnglishComments
    Deflection Temperature at 0.46 MPa (66 psi) 150 °C302 °FUnannealed; ASTM D648
    Deflection Temperature at 1.8 MPa (264 psi) 136 °C277 °FUnannealed; ASTM D648
    Vicat Softening Point 175 °C347 °FASTM D1525
    Flammability, UL94 HBHB

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Alcoa Deltalloy® 4032-T651 Aluminum
    Aluminum 4032-O
    LNP Lubricomp® DFL-4032 BK8-250 Polycarbonate, Glass Fiber Reinforcement, PTFE Lubricant
    Evonik DEGALAN® 4032 Methacrylic Polymer
    Aluminum 4032-T6

    PMULTI133 / 54037

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.