MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Aluminum 4032-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 4000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A94032; Aluminium 4032-O; AA4032-O; Al4032-O
Vendors: Eagle Alloys Corporation is a leading supplier of quality metals and alloys. Our staff prides itself on working fast, efficiently and courteously to get you the information you need. Call (800) 237-9012 or visit www.EagleAlloys.com.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.68 g/cc0.0968 lb/in³AA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000432 ohm-cm
@Temperature 20.0 °C
0.00000432 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  18.0 µm/m-°C
@Temperature -50.0 - 20.0 °C
10.0 µin/in-°F
@Temperature -58.0 - 68.0 °F
 19.4 µm/m-°C
@Temperature 20.0 - 100 °C
10.8 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 19.5 µm/m-°C
@Temperature 20.0 - 100 °C
10.8 µin/in-°F
@Temperature 68.0 - 212 °F
 20.2 µm/m-°C
@Temperature 20.0 - 200 °C
11.2 µin/in-°F
@Temperature 68.0 - 392 °F
 21.0 µm/m-°C
@Temperature 20.0 - 300 °C
11.7 µin/in-°F
@Temperature 68.0 - 572 °F
Thermal Conductivity 154 W/m-K1070 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 532 - 571 °C990 - 1060 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 532 °C990 °FAA; Typical
Liquidus 571 °C1060 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F2 to 3 hr at temperature then furnace cooled to 500°F at 50°F per hour max
Solution Temperature 504 - 516 °C940 - 960 °FHold 4 min at temperature then quench in cold water; for heavy or complicated forgings, quench in water at 150 to 212°F
Aging Temperature 168 - 174 °C335 - 345 °F8 to 12 hr at temperature
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 81.1 - 87.2 %81.1 - 87.2 %As remainder
Chromium, Cr <= 0.10 %<= 0.10 %
Copper, Cu 0.50 - 1.3 %0.50 - 1.3 %
Iron, Fe <= 1.0 %<= 1.0 %
Magnesium, Mg 0.80 - 1.3 %0.80 - 1.3 %
Nickel, Ni 0.50 - 1.3 %0.50 - 1.3 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si 11 - 13.5 %11 - 13.5 %
Zinc, Zn <= 0.25 %<= 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 4032-T6
Alcoa Deltalloy® 4032-T651 Aluminum
Aluminum 4045
Alcoa Deltalloy® 4032-T86 Aluminum
4047 Aluminum

MA4032O / 9079

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.