Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.21 g/cc | 1.21 g/cc |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 75 | 75 |
| 58 @Treatment Temp. 150 °C, Time 252000 sec | 58 @Treatment Temp. 302 °F, Time 70.0 hour |
| 71 @Treatment Temp. 150 °C, Time 252000 sec | 71 @Treatment Temp. 302 °F, Time 70.0 hour |
| 72 @Treatment Temp. 100 °C, Time 252000 sec | 72 @Treatment Temp. 212 °F, Time 70.0 hour |
| 75 @Treatment Temp. 175 °C, Time 252000 sec | 75 @Treatment Temp. 347 °F, Time 70.0 hour |
| 77 @Treatment Temp. 175 °C, Time 605000 sec | 77 @Treatment Temp. 347 °F, Time 168 hour |
Tensile Strength | 17.11 MPa | 2482 psi |
| 11.465 MPa @Treatment Temp. 150 °C, Time 252000 sec | 1662.9 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 16.925 MPa @Treatment Temp. 175 °C, Time 252000 sec | 2454.7 psi @Treatment Temp. 347 °F, Time 70.0 hour |
| 17.352 MPa @Treatment Temp. 150 °C, Time 252000 sec | 2516.7 psi @Treatment Temp. 302 °F, Time 70.0 hour |
| 17.643 MPa @Treatment Temp. 175 °C, Time 605000 sec | 2558.9 psi @Treatment Temp. 347 °F, Time 168 hour |
Elongation, Ultimate | 235 % | 235 % |
| 184.9 % @Treatment Temp. 150 °C, Time 252000 sec | 184.9 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 224 % @Treatment Temp. 175 °C, Time 252000 sec | 224 % @Treatment Temp. 347 °F, Time 70.0 hour |
| 224.9 % @Treatment Temp. 175 °C, Time 605000 sec | 224.9 % @Treatment Temp. 347 °F, Time 168 hour |
| 241.1 % @Treatment Temp. 150 °C, Time 252000 sec | 241.1 % @Treatment Temp. 302 °F, Time 70.0 hour |
50% Modulus | 2.95 MPa | 2.95 MPa |
100% Modulus | 7.219 MPa | 1047 psi |
Tear Strength | 35.9 kN/m | 205 pli |
| 45.6 kN/m | 260 pli |
Compression Set | 5.0 % @Treatment Temp. 175 °C, Time 79200 sec | 5.0 % @Treatment Temp. 347 °F, Time 22.0 hour |
| 6.7 % @Treatment Temp. 150 °C, Time 79200 sec | 6.7 % @Treatment Temp. 302 °F, Time 22.0 hour |
| 6.8 % @Treatment Temp. 175 °C, Time 79200 sec | 6.8 % @Treatment Temp. 347 °F, Time 22.0 hour |
| 7.4 % @Treatment Temp. 150 °C, Time 79200 sec | 7.4 % @Treatment Temp. 302 °F, Time 22.0 hour |
| 9.9 % @Treatment Temp. 175 °C, Time 252000 sec | 9.9 % @Treatment Temp. 347 °F, Time 70.0 hour |
| 12.2 % @Treatment Temp. 175 °C, Time 252000 sec | 12.2 % @Treatment Temp. 347 °F, Time 70.0 hour |
| 13.1 % @Treatment Temp. 150 °C, Time 252000 sec | 13.1 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 15.5 % @Treatment Temp. 150 °C, Time 252000 sec | 15.5 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 31.7 % @Treatment Temp. 150 °C, Time 2.59e+6 sec | 31.7 % @Treatment Temp. 302 °F, Time 720 hour |
|
Thermal Properties | Metric | English | Comments |
---|
Brittleness Temperature | -37.2 °C | -35.0 °F |
Shrinkage | 3.1 % @Treatment Temp. 100 °C, Time 252000 sec | 3.1 % @Treatment Temp. 212 °F, Time 70.0 hour |
| 7.4 % @Treatment Temp. 150 °C, Time 252000 sec | 7.4 % @Treatment Temp. 302 °F, Time 70.0 hour |
| 48.5 % @Treatment Temp. 150 °C, Time 252000 sec | 48.5 % @Treatment Temp. 302 °F, Time 70.0 hour |
|
Descriptive Properties |
---|
Color | Black |
TR-10 Temperature | -26°C |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.