MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Thermal Ceramics Kaolite 3300 High Temperature Insulating Castables
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Kaolite 3300 is a high strength bubble alumina, lightweight castable with a high-purity binder. It contains less than 0.2% iron oxide and 0.5% silica. Kaolite 3300 is recommended for transfer lines to secondary ammonia reformers, and other applications where resistance to hydrogen atmospheres and silica pickup is critical.

Features:

  • Low thermal conductivity
  • Reduction of the quantity of heat storage and heat transfer produce significant savings in fuel consumption
  • Temperature range up to 3300°F (1816°C)
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 1.474 - 1.586 g/ccFired
     
    Mechanical PropertiesOriginal ValueComments
    Modulus of Rupture 0.800 - 1.20 ksiDried 18-24 hours at 220°F; ASTM C133
     0.700 - 1.05 ksi
    @Treatment Temp. 816 °C,
    Time 18000 sec
    ASTM C133
     1.00 - 1.85 ksi
    @Treatment Temp. 1760 °C,
    Time 18000 sec
    ASTM C133
    Compressive Strength 15.9 - 23.4 MPaFired 5 hours at 1500°F
     17.2 - 24.1 MPaDried for 18-24 hours at 220°F
     20.7 - 27.6 MPaFired 5 hours at 3300°F
     
    Thermal PropertiesOriginal ValueComments
    Thermal Conductivity 7.30 BTU-in/hr-ft²-°F
    @Temperature 816 °C
    ASTM C417
     7.30 BTU-in/hr-ft²-°F
    @Temperature 1090 °C
    ASTM C417
     7.70 BTU-in/hr-ft²-°F
    @Temperature 1370 °C
    ASTM C417
     8.00 BTU-in/hr-ft²-°F
    @Temperature 538 °C
    ASTM C417
     9.90 BTU-in/hr-ft²-°F
    @Temperature 260 °C
    ASTM C417
    Maximum Service Temperature, Air 3300 °F
    Shrinkage 0.10 - 0.30 %
    @Temperature 816 °C,
    Time 18000 sec
    ASTM C113
     0.00 - 0.60 %
    @Temperature 1820 °C,
    Time 18000 sec
    ASTM C113
     0.00 - 0.20 %
    @Treatment Temp. 104 °C
    Dried 18-24 hours; ASTM C113
     
    Processing PropertiesOriginal ValueComments
    Shelf Life 12.0 Month
     
    Component Elements PropertiesOriginal ValueComments
    Al2O3 94 %
    Alkalis 0.50 %
    CaO 4.6 %
    Fe2O3 0.20 %
    MgO 0.10 %
    SiO2 0.50 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Thermal Ceramics Kaocast 3000 Dense Castable
    Morgan Advanced Ceramics Kaolite 3300 Thermal Ceramic
    Morgan Advanced Ceramics Kao-Tab® Monolithics 95 Thermal Ceramic
    Morgan Advanced Ceramics Alumor 90 Thermal Ceramic
    Thermal Ceramics Kaocrete HPM 90 Ultra High Strength Castables

    CTHERM062 / 2382

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.