MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
DSM Somos® 7110 Epoxy Photopolymer, Green Parts  (discontinued **)
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoset; Epoxy

Material Notes: Description

DSM Somos® 7110 Photopolymer is a humidity-tolerant, high heat-deflection-temperature, low-curl, high-speed liquid that produces rigid, highly accurate parts. It produces exceptional, undistorted thin walls and down-facing surfaces and exhibits good processing latitude.

Application

Somos® 7110 Photopolymer is used in the solid imaging process to build three-dimensional parts.

Information Provided by DSM Desotech Inc.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.


Axis Proto Inc. Innovative partners in producing fast Rapid Prototyping and short run manufacturing solutions using large scale 3D printing systems including SLA printing technology. Free 3D printing quotes at www.axisproto.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.13 g/cc
@Temperature 25.0 °C
Viscosity 700 cP
@Temperature 30.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 81ASTM D2240
Tensile Strength, Yield 44.0 MPaASTM D638M
Elongation at Break 4.7 - 7.4 %ASTM D638M
Modulus of Elasticity 1.758 GPaASTM D638M
Flexural Strength 59.0 MPaASTM D790M
Flexural Modulus 1710 MPaASTM D790M
Izod Impact, Notched 0.262 J/cmASTM D256A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 45.0 - 54.0 °CASTM D648
 
Descriptive Properties
AppearanceTransparent Amber
Dp (mm)0.14Slope of cure-depth vs. ln(E) curve
E10 (mJ/cm2)51Exposure that gives 0.254mm thickness
E5 (mJ/cm2)20Exposure that gives 0.127mm thickness
Ec (mJ/cm2)8.2Critical exposure

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Impact Grade
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded
DSM Somos® ProtoGen™ 18920 Liquid Photopolymer, UV Postcure at HOC +3
DSM Somos® ProtoGen™ 18920 Liquid Photopolymer, UV & Thermal Postcure
DSM Somos® ProtoCast™ AF 19122 Antimony-free Liquid Photopolymer

PDSMT032 / 93552

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.